Spectroscopic Ellipsometry of Nanocrystalline Diamond Film Growth
At a Glance
Section titled “At a Glance”| Metadata | Details |
|---|---|
| Publication Date | 2017-10-16 |
| Journal | ACS Omega |
| Authors | Evan L. H. Thomas, Soumen Mandal, Ashek-I-Ahmed Ashek-I-Ahmed, J. Emyr Macdonald, Thomas G. Dane |
| Institutions | University of Bristol, National Dong Hwa University |
| Citations | 25 |
| Analysis | Full AI Review Included |
Technical Analysis of Early-Stage Nanocrystalline Diamond Growth Characterized via Spectroscopic Ellipsometry
Section titled “Technical Analysis of Early-Stage Nanocrystalline Diamond Growth Characterized via Spectroscopic Ellipsometry”Executive Summary
Section titled “Executive Summary”- Objective: Characterizes the initial stages of nanocrystalline diamond (NCD) film growth on silicon substrates using ex situ Spectroscopic Ellipsometry (SE) to decouple nucleation, coalescence, and bulk growth regimes.
- Substrate Prep: Utilizes electrostatic self-assembly of hydrogen-terminated nanodiamond colloids (4-8 nm particles) on p-type Si(100) wafers, achieving ultra-high seeding densities exceeding 1011 cm-2.
- Growth Method: Conducts Microwave Plasma Chemical Vapor Deposition (MPCVD) using an Astex AX6500 reactor with a two-stage gas recipe: a high methane fraction (3.86% CH4/H2) for initial stabilization, followed by a low fraction (0.6% CH4/H2) for high-quality bulk NCD.
- Key Modeling Achievement: Successfully applies a Bruggeman Effective Medium Approximation (EMA) to quantify the diamond (Di), glassy carbon (g-C), and void fractions, tracking the evolution from isolated Van der Drift (VW) islands to a fully coalesced, columnar film.
- Interfacial Insights: Quantifies the formation and stabilization of an interfacial β-SiC layer (peaking at ~8.9 nm before settling at ~5.5 nm) formed via plasma diffusion and substrate etching.
- Correlation: Cross-validates SE optical modeling with Atomic Force Microscopy (AFM), Scanning Electron Microscopy (SEM), Raman Spectroscopy, and Grazing Incidence X-Ray Diffraction (GIXRD).
Technical Specifications
Section titled “Technical Specifications”| Parameter | Value | Unit | Context |
|---|---|---|---|
| Substrate | Si(100), p-type | - | 2-inch wafers, <0.005 Ω·cm resistivity, 500 µm thick |
| Seeding Density | > 1011 | cm-2 | Achieved via electrostatic self-assembly |
| Seed Particle Size | 4 - 8 | nm | Monodispersed nanodiamond colloid |
| Initial CH4 Fraction | 3.86 | % | First 3 minutes to prevent seed etching |
| Bulk CH4 Fraction | 0.6 | % | Remainder of growth for high-quality NCD |
| Process Pressure | 40 | Torr | Maintained throughout deposition |
| Microwave Power | 3.5 | kW | Astex AX6500 reactor |
| Substrate Temperature | ~860 | °C | Measured via dual-wavelength pyrometry |
| Max Growth Duration | 123 | min | Evaluated across 4, 6, 8, 13, 20, 30, 40, and 123 min |
| Seed EMA Thickness | 4.38 | nm | Composed of 54.9% void and 4.5% g-C |
| Peak SiC Interlayer Thickness | 8.85 | nm | Observed at 8 min growth duration |
| Steady-State SiC Thickness | 5.03 - 6.7 | nm | Stable plateau for 20 - 123 min durations |
| Bulk Thickness (40 min) | 79.3 | nm | Rapid increase following coalescence |
| Bulk g-C Content (40 min) | 22.7 | % | Peak non-diamond carbon content |
| Bulk Void Fraction (40 min) | 7.4 | % | Parabolic decrease during lateral growth |
| EL Wavelength Range | 1.2 - 6.2 | eV | Equivalent to 200 - 1000 nm |
| EL Incidence Angles | 65, 70, 75 | ° | Multi-angle data acquisition |
| Raman Laser Excitation | 488 | nm | 0.5 mW power, 30 s acquisition time |
| XRD Beamline Energy | 12.5 | keV | Diamond Light Source beamline I07 |
Key Methodologies
Section titled “Key Methodologies”- Substrate Preparation:
- Immerse Si(100) wafers in a hydrogen-terminated nanodiamond/DI water colloid.
- Subject to ultrasonic agitation for 10 minutes to drive electrostatic self-assembly.
- Rinse and spin-dry prior to loading into the CVD chamber.
- MPCVD Growth Protocol:
- Load seeded substrates into an Astex AX6500 reactor.
- Phase 1 (Nucleation Stabilization): Flow 3.86% CH4 in H2 for the first 3 minutes to stabilize the ~5 nm seeds against plasma etching.
- Phase 2 (Bulk Growth): Reduce methane fraction to 0.6% in H2 for the remainder of the cycle.
- Maintain chamber pressure at 40 Torr and microwave power at 3.5 kW, yielding a substrate temperature of ~860 °C.
- Cool samples in a pure H2 plasma to prevent the formation of non-sp3-bonded carbon.
- Spectroscopic Ellipsometry (SE) Modeling:
- Acquire spectra using a J.A. Woollam M-2000D rotating compensator ellipsometer.
- Incorporate a 5 nm instrument bandwidth to account for depolarization from thickness nonuniformity.
- Fit data using a Bruggeman Effective Medium Approximation (EMA) combining diamond, glassy carbon (g-C), and void.
- Model the interfacial carbide layer using reference optical constants for β-SiC.
- Correlative Validation:
- Use non-contact AFM (Park Systems XE-100) to validate surface roughness and grain morphology.
- Use Raman spectroscopy (488 nm laser) to verify sp3/sp2 ratios and grain boundary content (1150 cm-1 TPA peak).
- use GIXRD (0.4° incidence) to confirm crystalline quality and phase purity.
6CCVD Solutions & Capabilities
Section titled “6CCVD Solutions & Capabilities”The methodologies and characterization pathways detailed in this study highlight the critical importance of precise interface engineering and early-stage growth control. 6CCVD provides the materials and customization required to extend these fundamental findings into applied devices.
-
Applicable Materials:
- Optical Grade Single Crystal Diamond (SCD): For applications requiring bulk-like optical constants without the grain boundary phonon absorption at 1150 cm-1 seen in NCD films.
- Nanocrystalline / Polycrystalline Diamond (PCD): 6CCVD produces freestanding PCD wafers up to 125mm with thicknesses spanning 0.1µm to 500µm, ideal for substrates requiring the columnar grain structures analyzed in this paper.
- Heavy Boron Doped PCD (BDD): For electrochemical or MEMS resonator applications where interfacial conductivity and grain boundary management are critical. Our BDD films offer precise control over sp2 content and surface morphology.
-
Customization Potential:
- The paper details a complex multilayer stack (SiC interlayer, diamond bulk, surface roughness). 6CCVD offers custom metalization (Au, Pt, Pd, Ti, W, Cu) to address the interfacial resistance challenges and Schottky barrier formations inherent to diamond-on-silicon architectures.
- We provide laser cutting and dicing services to deliver custom geometries, bypassing the need for mechanical scribing (as used in the paper’s 1 x 1 cm2 sample prep) which can introduce edge defects.
- 6CCVD can supply diamond substrates polished to Ra < 5nm (for inch-size PCD) and Ra < 1nm (for SCD), enabling reproducible SE modeling and minimizing surface roughness variability.
-
Engineering Support:
- Our in-house PhD engineering team specializes in tailoring MPCVD recipes to manipulate the delicate balance between the gas-phase chemistry and the substrate interface. We can assist in optimizing CH4/H2 ratios, seeding densities, and cooling protocols to stabilize the β-SiC interfacial layer or promote lateral Van der Drift growth for specific MEMS or tribological applications.
- Whether transitioning from planar silicon substrates to complex 3D architectures or scaling up from 2-inch wafers to 125mm plates, our team provides consultative support for material selection and integration.
-
Call to Action:
- For custom specifications, specialized metalization, or material consultation on diamond-substrate interfaces, visit 6ccvd.com or contact our engineering team directly. Global shipping is available (DDU default, DDP optional) to support your research and production timelines.
View Original Abstract
With the retention of many of the unrivaled properties of bulk diamond but in thin-film form, nanocrystalline diamond (NCD) has applications ranging from micro-/nano-electromechanical systems to tribological coatings. However, with Young’s modulus, transparency, and thermal conductivity of films all dependent on the grain size and nondiamond content, compositional and structural analysis of the initial stages of diamond growth is required to optimize growth. Spectroscopic ellipsometry (SE) has therefore been applied to the characterization of 25-75 nm thick NCD samples atop nanodiamond-seeded silicon with a clear distinction between the nucleation and bulk growth regimes discernable. The resulting presence of an interfacial carbide and peak in nondiamond carbon content upon coalescence is correlated with Raman spectroscopy, whereas the surface roughness and microstructure are in accordance with values provided by atomic force microscopy. As such, SE is demonstrated to be a powerful technique for the characterization of the initial stages of growth and hence the optimization of seeding and nucleation within films to yield high-quality NCD.