Precision micro-mechanical components in single crystal diamond by deep reactive ion etching
At a Glance
Section titled “At a Glance”| Metadata | Details |
|---|---|
| Publication Date | 2018-06-08 |
| Journal | Microsystems & Nanoengineering |
| Authors | Adrien Toros, Marcell Kiss, Teodoro Graziosi, Hamed Sattari, P. Gallo |
| Institutions | Y-Parc (Switzerland), École Polytechnique Fédérale de Lausanne |
| Citations | 53 |
| Analysis | Full AI Review Included |
Executive Summary
Section titled “Executive Summary”- Breakthrough Fabrication Technique: Demonstrates fully released, freestanding micro-mechanical components (e.g., watch escape wheels and anchors) precision-structured entirely in 150 µm-thick Single Crystal Diamond (SCD) via deep reactive ion etching (DRIE).
- Optimized Hard Mask Stack: Overcomes micromasking and delamination through a novel 3-layer mask structure: a 200 nm Al adhesion layer, a 65 nm SiO2 stress buffer, and a 7 µm bulk SiO2 layer sputtered with and without O2.
- High-Performance Etch Recipe: Achieves a record-high etch rate of >30 µm/h with a hard mask selectivity better than 1:50, using a highly biased, high-intensity pure oxygen plasma.
- Geometric Precision: Delivers highly anisotropic sidewall profiles between 82° and 93°, with sidewall surface roughness better than 200 nm RMS—a >5× improvement over femtosecond laser structuring.
- Novel Photolithography Workflow: Implements a two-cycle exposure technique to completely remove the photoresist edge-bead on small (<6 mm) substrates, ensuring high-fidelity pattern transfer without pick-and-place limitations.
- Application Versatility: Provides a manufacturing pathway for monolithic diamond MEMS, optical components (lenses, gratings), and high-precision timekeeping mechanisms demanding extreme hardness and low friction.
Technical Specifications
Section titled “Technical Specifications”| Parameter | Value | Unit | Context |
|---|---|---|---|
| Substrate Material | Single Crystal Diamond (SCD) | — | CVD-grown, high-purity, mechanical grade |
| Substrate Dimensions | 5.5 × 5.5 × 150 | µm | Initial handling size prior to dicing |
| Component Thickness | 150 | µm | Fully etched through-wafer thickness |
| Diamond Etch Rate | >30 | µm/h | Achieved via high-bias oxygen plasma |
| Hard Mask Selectivity | 1:50 | — | Diamond etch rate vs. SiO2 mask consumption |
| Hard Mask Material | SiO2 (on Al adhesion) | — | 7 µm total thickness, RF sputtered |
| Adhesion Layer | Aluminum (Al) | — | 200 nm thick, front and backside |
| Etch Plasma Chemistry | Pure Oxygen (O2) | — | High-density, highly anisotropic plasma |
| Sidewall Angle | 82° - 93° | ° | Measured post-etch profile |
| Sidewall Roughness | <200 (up to 20) | nm RMS | Over 5 µm × 5 µm areas (post plane-fitting) |
| Surface Smoothness Gain | 5× to 50× | — | Improvement vs. 1.2 mm femtosecond laser parts |
| Photoresist Thickness | 2.5 | µm | Spin-coated for lithography exposure |
| Edge-Bead Removal | Two-cycle exposure | — | Custom lithography technique for small dies |
Key Methodologies
Section titled “Key Methodologies”- Substrate Preparation: Start with a high-purity, single-side polished SCD plate sized at 5.5 mm × 5.5 mm × 150 µm.
- Hard Mask Deposition:
- Adhesion Layer: Deposit 200 nm of Al on the diamond frontside via evaporation/sputtering.
- Buffer Layer: Sputter 65 nm of SiO2 using an Ar + O2 gas mixture to reduce internal stress.
- Bulk Mask: Sputter an additional ~7 µm of SiO2 using pure Ar to achieve practical deposition rates.
- Sacrificial Layer: Deposit an identical 200 nm Al layer on the diamond backside for later component release.
- Carrier Bonding: Temporarily mount the diamond plate onto a 4-inch Si handling wafer using mounting wax to enable standard microfabrication tooling.
- Edge-Bead Lithography: Spin-coat a 2.5 µm photoresist layer. Execute a two-cycle UV exposure—first exposing a 0.5 mm-wide frame at the edges with a high dose, developing, then performing the primary pattern exposure.
- Mask Patterning: Pattern and develop the photoresist, then transfer the geometry into the thick SiO2 hard mask (e.g., via CHF3/Ar RIE).
- Diamond DRIE: Perform high-density, highly biased pure O2 reactive ion etching. Etch completely through the 150 µm substrate at >30 µm/h.
- Component Release: Chemically or electrochemically etch the sacrificial backside Al layer using an appropriate solvent/acid to release the freestanding diamond components.
6CCVD Solutions & Capabilities
Section titled “6CCVD Solutions & Capabilities”This research highlights the critical intersection of high-quality bulk diamond and complex micro-fabrication. Achieving such precision requires starting materials that are uniformly defect-free and dimensionally exact. Below is how 6CCVD directly supports these engineering challenges.
-
Applicable Materials:
- Optical & Mechanical Grade SCD: The 150 µm through-etch process demands high-purity single crystal diamond with minimal crystal defects to prevent etch pitting and ensure structural integrity. 6CCVD provides ultra-flat, single crystal diamond (SCD) wafers and plates specifically engineered for MEMS, optical, and quantum applications.
- Boron-Doped SCD (BDD): For applications requiring tunable conductivity during plasma etching or for integrated diamond electrodes, our boron-doped single crystal diamond offers precise dopant control without sacrificing the crystalline structure.
-
Customization Potential:
- Precision Thickness Control: The paper specifies a strict 150 µm thickness requirement. 6CCVD specializes in custom diamond thicknesses ranging from 0.1 µm to 500 µm for SCD, allowing engineers to optimize their DRIE recipes for shallower cantilevers or deeper watch mechanisms.
- Wafer Scaling: While the paper notes limitations with 5.5 mm × 5.5 mm substrates (edge-bead effects), 6CCVD provides SCD and PCD plates up to 125 mm, enabling high-volume, parallelized manufacturing on a wafer-scale level.
- Surface Engineering: Sidewall roughness (200 nm RMS) is heavily dependent on initial substrate quality. 6CCVD offers precision polishing with surface roughness down to Ra < 1 nm, providing an ideal starting surface for lithography and reducing downstream etching variables.
- Custom Metalization: For researchers requiring bespoke electrode integration or hard mask adhesion layers, our in-house metalization capabilities include Au, Pt, Pd, Ti, W, and Cu, ensuring perfect adhesion and patterning compatibility.
-
Engineering Support:
- Specifying the exact diamond grade, crystal orientation (e.g., <100> vs. <111>), and thickness is paramount for successful deep RIE. 6CCVD’s in-house PhD engineering team provides direct material consultation to optimize your substrate selection for high-aspect-ratio etching, minimizing micromasking effects and maximizing yield.
-
Call to Action:
- For custom specifications, specific crystal orientations, or material consultation for your MEMS and micro-mechanical projects, visit 6ccvd.com or contact our engineering team directly.
View Original Abstract
Abstract The outstanding material properties of single crystal diamond have been at the origin of the long-standing interest in its exploitation for engineering of high-performance micro- and nanosystems. In particular, the extreme mechanical hardness, the highest elastic modulus of any bulk material, low density, and the promise for low friction have spurred interest most notably for micro-mechanical and MEMS applications. While reactive ion etching of diamond has been reported previously, precision structuring of freestanding micro-mechanical components in single crystal diamond by deep reactive ion etching has hitherto remained elusive, related to limitations in the etch processes, such as the need of thick hard masks, micromasking effects, and limited etch rates. In this work, we report on an optimized reactive ion etching process of single crystal diamond overcoming several of these shortcomings at the same time, and present a robust and reliable method to produce fully released micro-mechanical components in single crystal diamond. Using an optimized Al/SiO2hard mask and a high-intensity oxygen plasma etch process, we obtain etch rates exceeding 30 µm/h and hard mask selectivity better than 1:50. We demonstrate fully freestanding micro-mechanical components for mechanical watches made of pure single crystal diamond. The components with a thickness of 150 µm are defined by lithography and deep reactive ion etching, and exhibit sidewall angles of 82°-93° with surface roughness better than 200 nm rms, demonstrating the potential of this powerful technique for precision microstructuring of single crystal diamond.
Tech Support
Section titled “Tech Support”Original Source
Section titled “Original Source”References
Section titled “References”- 2013 - Optical Engineering of Diamond [Crossref]