AnalysisFull AI Review Included
  • Demonstrates 3 GHz RF Load-Pull Performance: AlGaN/GaN HEMTs transferred from native Si substrates to single crystalline diamond (SCD) exhibit a 15% increase in maximum output power density (Pout) and a 14% increase in Power Added Efficiency (PAE) compared to identical devices on Si.
  • Low-Temperature Direct Bonding: A 30 nm aluminum hydroxide bond layer formed via hydrothermal conversion enables the transfer of prefabricated GaN devices onto diamond at temperatures compatible with the semiconductor process (< 300 °C).
  • Thermal Management Validation: COMSOL Multiphysics simulations correlate the device performance enhancement to a calculated channel temperature reduction of approximately 100 K when moving from Si to SCD substrates.
  • Power Scalability Across Gate Fingers: The Pout of a 6 × 300 µm transistor (8.0 W/mm) matches the 2 × 300 µm transistor, confirming uniform lateral heat spreading across the 60 µm inter-finger distance.
  • Record Total Output Power: A 14.4 W continuous-wave (cw) total output power is achieved from a single GaN-on-SCD device at 55 V drain bias.
  • Identifies Buffer Thermal Bottleneck: The superlattice (SL) buffer remains the primary thermal resistance; improvements in the bond interface yield diminishing returns until the buffer is optimized or removed.
  • Process Compatibility: The technique is substrate-agnostic and has been validated for GaN-on-glass, SiC, sapphire, polycrystalline diamond, and single crystalline diamond.
ParameterValueUnitContext
Operating Frequency3GHzRF load-pull measurement frequency
VDS (Peak)70VMaximum tested drain-source bias before breakdown (pulsed)
VDS (Continuous Max)55VHighest sustained cw operation for 6 × 300 µm device
Maximum Pout (2 × 300 µm, 70 V)10.0W/mmPulsed, pre-breakdown
Maximum Pout (2 × 300 µm, 50 V, cw)7.8W/mmContinuous wave on SCD
Maximum Pout (6 × 300 µm, 55 V, cw)8.0W/mmContinuous wave on SCD
Maximum Pout (6 × 300 µm, 55 V, pulsed)8.8W/mmPulsed measurement on SCD
Total RF Power (6 × 300 µm, 55 V, cw)14.4WLargest reported for GaN-on-diamond
PAE (50 V, cw)55 - 58%SCD device vs. 51% on Si (+14%)
Gate Length500nmEstimated peak field: ~1.4 MV/cm at 70 V
Gate Pitch60µmInter-finger thermal isolation distance
Gate Width300µmPer finger
Calculated Tchannel Reduction~100KSCD vs. Si substrate at same Pout
Layer StackSiN (200 nm) / GaN (800 nm) / SL (2 µm) / AlN (150 nm)—Epitaxial structure on transferred film
Bond Layer Thickness30nmAluminum hydroxide (Al(OH)x)
κ (GaN thin film)185W·m-1·K-1At 300 K, α = -1.42
Critical Field (GaN)3.3MV/cmMaterial limit for breakdown
  1. Epitaxial Growth: AlGaN/GaN heterostructure with 2 µm superlattice (SL) buffer and 150 nm AlN nucleation layer grown on 150 mm Si substrate.
  2. Device Fabrication: Standard HEMT processing on the Si substrate; gate length 500 nm, gate widths of 300 µm per finger, with 2-finger and 6-finger variants.
  3. Direct Low-Temperature Bonding: A thin water film is sandwiched between the fabricated GaN device surface and the diamond substrate; hydrothermal conversion at temperatures < 300 °C dissolves a thin AlN layer and re-crystallizes aluminum hydroxides (Al(OH)3), forming a ~30 nm bond interface.
  4. Substrate Removal: The Si growth substrate is removed, leaving the AlGaN/GaN thin film bonded directly to SCD; the original buffer/nucleation layers can be mechanically/chemically thinned or removed.
  5. RF Characterization: 3 GHz load-pull measurements in both continuous wave (cw) and pulsed (10 µs) modes across drain voltages from 50 V to 70 V.
  6. Thermal Simulation: COMSOL Multiphysics finite element analysis using temperature-dependent thermal conductivity κ(T) = κ300·(T/300)α; a planar heat source equal to measured Pout is applied at the gate region.
  7. Thermal Model Materials: GaN κ = 185 W·m-1·K-1, α = -1.42; AlN/SL buffer treated as dominant phonon-scattering interface resistance.
Requirement in Paper6CCVD Recommendation
Single Crystalline Diamond (SCD) substrate for GaN transferOptical Grade SCD plates, polished to Ra < 1 nm, with thickness range 0.1-500 µm to match thermal management layer requirements
Alternative polycrystalline diamond optionElectronic Grade PCD (inch-size, polished Ra < 5 nm) for cost-effective GaN-on-diamond integration
Boron-doped option for tailored thermal/electrical interfaceHeavy Boron-Doped PCD (BDD) with metallization-ready surface for hybrid GaN-diamond co-design
  • Custom Dimensions: 6CCVD supplies diamond plates/wafers up to 125 mm in diameter — directly compatible with 150 mm GaN-on-Si fab process flows when diced or adapted to standard 3-inch/4-inch pockets.
  • Bond-Ready Surface: Surface preparation suitable for hydrophilic bonding (analogous to the Al(OH)x bond layer described), with sub-nanometer roughness certification provided with every shipment.
  • Custom Metallization: The paper implies eventual integration with metal contact layers. 6CCVD’s in-house Ti / Pt / Au / W / Cu deposition capability supports back-side metallization, ground planes, and laser-cut via geometries for advanced package-level thermal stacks.
  • Laser Cutting & Dicing: Custom-shaped substrates for matched thermal expansion mounting, available through laser micro-machining services.

The GaN-on-diamond integration pathway described in this paper requires careful matching of diamond surface energy, thermal expansion coefficient, and bond-process temperature window. 6CCVD’s in-house PhD engineering team is available to assist with:

  • Material selection (SCD vs. PCD vs. BDD) for specific RF power density targets.
  • Surface preparation specifications tuned to the target bonding chemistry (hydrothermal, eutectic, or sputtered interface).
  • Co-design of metallization stacks for subsequent GaN epilayer bonding or direct die-attach applications.
  • Thermal simulation parameter validation using measured κ(T) curves for supplied substrates.

For custom specifications or material consultation, visit 6ccvd.com or contact our engineering team directly. Global shipping is available with DDU as the default Incoterm and DDP on request.

View Original Abstract

The integration of AlGaN/GaN thin film transistors onto diamond substrates enables the efficient dissipation of device heat, thus providing a boost in performance and reliability of current high-frequency GaN power amplifiers. In this paper, we show 3 GHz load-pull measurements of GaN transistors on silicon (Si) and single crystalline diamond (SCD) as fabricated by our recently presented direct low-temperature bond process. After the transfer onto SCD, the efficiency and output power are increased by 15%, which is explained by a calculated temperature difference of ∼100 K. In addition, the temperature between individual gate fingers is reduced such that the output power density (Pout) is independent of the amount of fingers. A drawback of our GaN epilayer is identified in the huge thermal resistance of the buffer layer so that the heat spreading performance of our technology is significantly impaired. Nevertheless, we demonstrate a large GaN-on-diamond output power of 14.4 W at a Pout of 8.0 W/mm.