Microstructures Manufactured in Diamond by Use of Laser Micromachining.
At a Glance
Section titled “At a Glance”| Metadata | Details |
|---|---|
| Publication Date | 2020-03-06 |
| Journal | Apollo (University of Cambridge) |
| Authors | Dudek, Rosowski, Kozanecki, Jaszczak, Szymański |
| Citations | 1 |
| Analysis | Full AI Review Included |
Executive Summary
Section titled “Executive Summary”- Demonstrated Process: High-precision laser micromachining of bulk polycrystalline diamond (PCD) using a 355 nm DPSS laser for microfluidic and MEMS prototyping.
- Material Source: The 530 µm free-standing PCD plate was produced via MW PECVD (DF-100 system, 2% CH4/H2, 87 Torr, 820 °C).
- Optimal Microstructure Parameters: Achieved grooves of 12.8 µm width and 245 µm depth, with wall slopes reaching 88.9° and roughness Ra 0.135 µm.
- Phase Control Capability: Demonstrated precise control over material phase — preserving the sp3 diamond signature (1332 cm−1 band) versus inducing controlled graphitization (D/G peaks at 1350 and 1580 cm−1) through scan-speed tuning.
- Key Insight: Higher scan speeds (400 mm/s) and pulse overlap (above 50%) drive localized graphitization, while slow speeds (100 mm/s) with 5 µm hatch spacing preserve bulk diamond integrity.
- Application Impact: Validates diamond as a viable substrate for MEMS and microfluidic devices requiring precise 3D structuring.
Technical Specifications
Section titled “Technical Specifications”| Parameter | Value | Unit | Context |
|---|---|---|---|
| Diamond Thickness | 530 | µm | Free-standing PCD plate |
| Microwave Power (Deposition) | 3.6 | kW | MW PECVD growth |
| Methane Content | 2 | % | CH4/H2 ratio |
| Total Gas Flow | 800 | sccm | Process gas mixture |
| Deposition Pressure | 87 | Torr | Chamber pressure |
| Substrate Temperature | 820 | °C | Growth temperature |
| Growth Rate | 1 | µm/h | Deposition rate |
| Hardness | 85.1 ± 10.2 | GPa | Vickers indentation |
| Young’s Modulus | 1114.5 ± 183.8 | GPa | Mechanical stiffness |
| Thermal Conductivity | 1040 / 1280 | W m-1 K-1 | Two measured samples |
| Laser Wavelength | 355 | nm | DPSS UV source |
| Pulse Repetition Rate | 50 | kHz | Nanosecond pulses |
| Average Power Range | 5 to 11 | W | Tested power window |
| Pulse Duration | 25-35 | ns | Varies with frequency/power |
| Scan Speed Range | 50 to 400 | mm/s | Affects pulse overlap |
| Hatching Distance | 5 to 20 | µm | Inter-line spacing |
| Optimal Groove Width | 12.8 | µm | Narrowest achieved |
| Maximum Groove Depth | 245 | µm | Deepest achieved |
| Groove Wall Slope | ≥88.9 | ° | Near-vertical geometry |
| Surface Roughness (Ra) | 0.135 | µm | Smoothest region |
| Diamond Raman Peak (as-deposited) | 1332.9 | cm-1 | Reference |
| FWHM (as-deposited) | 4.1 | cm-1 | Baseline quality |
| Diamond Peak Shift at 9.5 W | 1331.3 | cm-1 | Post-laser modification |
| D Peak Position | ~1350 | cm-1 | Graphite signature |
| G Peak Position | ~1580 | cm-1 | Graphite signature |
| Hatching Direction | 0° and 90° | ° | Bidirectional grid |
| Purge Gas | None | — | Process atmosphere |
Key Methodologies
Section titled “Key Methodologies”- Substrate Preparation: Si wafer seeded with detonation nanodiamond suspension in ethanol via ultrasonic bath prior to deposition.
- Diamond Deposition: MW PECVD (DF-100) at 3.6 kW, 2% CH4/H2, 800 sccm, 87 Torr, 820 °C substrate temp; 530 µm thick free-standing PCD plate recovered.
- Laser Source: DPSS UV laser (Coherent AVIA), 355 nm wavelength, 50 kHz pulse repetition, 25-35 ns pulse duration.
- Scanning System: Galvanometer scanner delivering bi-directional hatching at 0°/90° cross-hatch pattern.
- Parameter Sweep: Average power varied 5-11 W; scan speed varied 50-400 mm/s; hatching distance varied 5-20 µm.
- Characterization Stack: Confocal laser scanning microscopy (Nikon MA200) for geometry, SEM (Hitachi S-3000N) for surface morphology, and Raman spectroscopy (Jobin-Yvon T-64000, 514.5 nm Ar excitation) for phase identification.
- Optimal Recipe Identified: 9.5 W average power, 100 mm/s scan speed, 5 µm hatching distance — produced narrowest grooves without hillocks and minimal graphitization.
6CCVD Solutions & Capabilities
Section titled “6CCVD Solutions & Capabilities”This research demonstrates that precision laser micromachining of PCD opens pathways to high-value MEMS, microfluidics, and photonic devices. 6CCVD offers the production-scale materials foundation required to replicate and extend this work.
-
Applicable Materials:
- Optical Grade PCD plates (0.1 µm to 500 µm thickness range; substrates up to 10 mm) — ideal for replicating the 530 µm free-standing plates used in this study and beyond. 6CCVD’s MPCVD PCD provides consistent grain structure essential for predictable laser ablation behavior.
- Single Crystal Diamond (SCD) — recommended for next-stage experiments requiring sub-micron surface roughness (Ra < 1 nm achievable via 6CCVD polishing) and uniform laser interaction without grain-boundary effects.
- Heavy Boron-Doped PCD (BDD) — for applications requiring the conductive graphitized microchannels demonstrated in this paper, where the original sp3 structure transitions to conductive sp2 carbon.
-
Customization Potential:
- Custom Dimensions: Plates and wafers up to 125 mm diameter available, enabling larger device arrays and microfluidic network prototyping beyond the lab-scale single-plate format.
- Custom Metalization: When integrating diamond microchannels into functional MEMS or electrochemical cells, 6CCVD’s in-house Au, Pt, Pd, Ti, W, and Cu metalization capabilities eliminate the need to source metallization from third parties — critical for sealed microfluidic interfaces.
- Laser Cutting Services: 6CCVD can pre-cut or post-cut diamond plates to your CAD specifications, reducing downstream machining time and ensuring consistent base geometry for laser micromachining workflows.
-
Engineering Support:
- 6CCVD’s in-house PhD team can assist with material selection for MEMS, microfluidic, and biomedical diamond applications. Whether your work targets electrophoretic separation chips, Joule-heated microdevices, or photonic structures, we provide guidance on optimal grain size, thickness, and surface finish for your specific laser-processing recipe.
-
Call to Action: For custom specifications or material consultation, visit 6ccvd.com or contact our engineering team directly.
View Original Abstract
Different microstructures were created on the surface of a polycrystalline diamond plate (obtained by microwave plasma-enhanced chemical vapor deposition-MW PECVD process) by use of a nanosecond pulsed DPSS (diode pumped solid state) laser with a 355 nm wavelength and a galvanometer scanning system. Different average powers (5 to 11 W), scanning speeds (50 to 400 mm/s) and scan line spacings (“hatch spacing”) (5 to 20 µm) were applied. The microstructures were then examined using scanning electron microscopy, confocal microscopy and Raman spectroscopy techniques. Microstructures exhibiting excellent geometry were obtained. The precise geometries of the microstructures, exhibiting good perpendicularity, deep channels and smooth surfaces show that the laser microprocessing can be applied in manufacturing diamond microfluidic devices. Raman spectra show small differences depending on the process parameters used. In some cases, the diamond band (at 1332 cm-1) after laser modification of material is only slightly wider and shifted, but with no additional peaks, indicating that the diamond is almost not changed after laser interaction. Some parameters did show that the modification of material had occurred and additional peaks in Raman spectra (typical for low-quality chemical vapor deposition CVD diamond) appeared, indicating the growing disorder of material or manufacturing of the new carbon phase.