Dislocation generation mechanisms in heavily boron-doped diamond epilayers
At a Glance
Section titled “At a Glance”| Metadata | Details |
|---|---|
| Publication Date | 2021-02-01 |
| Journal | Applied Physics Letters |
| Authors | D. Araújo, Fernando Lloret, Gonzalo Alba, M. P. Alegre, M.P. Villar |
| Institutions | Universidad de Cádiz |
| Citations | 14 |
| Analysis | Full AI Review Included |
Executive Summary
Section titled “Executive Summary”- Core Objective: Establishes empirical rules to suppress dislocation generation in heavily boron-doped diamond (BDD) epilayers grown by MPCVD, a critical issue for high-power, high-frequency, and radiation-hard electronics.
- Key Discovery: A “proximity effect” mechanism, unique to diamond, generates dislocations when two boron atoms occupy adjacent substitutional sites, independent of classical lattice strain relaxation.
- Critical Parameter Mapping: Quantifies a Critical Boron Level (CBL) governed by growth orientation ([100] vs. [111]) and CH4/H2 ratio, defining a safe process window below the People and Bean (P-B) critical thickness (hc).
- Experimental Validation: TEM analysis confirms dislocation-free epilayers for thicknesses of 10-50 nm at [B] = 2 × 1021 cm-3 when growth parameters fall within the dislocation-free region.
- Defect Engineering: Differentiates “killer” vs. “non-killer” dislocations and explains their spatial distribution using Peach-Koehler forces and energy balance models (Matthews-Blakeslee, People-Bean, Van der Merwe).
- Practical Outcome: Provides a process design map (doping level vs. thickness vs. growth orientation) for fabricating high-crystalline-quality doped diamond suitable for diodes and transistors.
Technical Specifications
Section titled “Technical Specifications”| Parameter | Value | Unit | Context |
|---|---|---|---|
| Substrate | HPHT undoped diamond (Type IIa) | — | Typical TD density < 4 dislocations/cm2 |
| Growth Method | Microwave Plasma Enhanced CVD (MPCVD) | — | Homoepitaxial deposition |
| Doping Gas Source | Boron (e.g., B2H6 or trimethylboron) | — | Substitutional lattice incorporation |
| Doping Level (Tested) | Up to 2 × 1021 | cm-3 | ”Heavily doped” regime for p++ layers |
| Critical Boron Level ([100]) | 25 - 32 × 1020 | cm-3 | CBL for [100] orientation |
| Critical Boron Level ([111]) | 6.5 - 17 × 1020 | cm-3 | CBL for [111] orientation (lower tolerance) |
| CH4/H2 Ratio Range | 0.15 - 4 | % | Critical parameter governing CBL |
| Diamond Lattice Constant (a0) | 0.3566 | nm | Used in critical thickness calculations |
| Poisson Ratio (ν) | 0.2 | — | Diamond-specific parameter |
| Burger Vector (b, edge) | ≈ a0 = 0.3566 | nm | Edge dislocation magnitude |
| Epilayer Thickness Range | 10 - 500 | nm | Tested below/above P-B hc |
| Lattice Mismatch Range | 0 - 2 | % | Linear regime (below 2% at.) |
| P-B Critical Thickness (at [B]=1021 cm-3) | > 10 | µm | Rarely exceeded in standard MPCVD |
| Characterization Technique | TEM (DF, HAADF) | — | Zone axes: [004], [011], [001] |
| Growth Modes | 2D layer-by-layer; lateral (ICP terrace) | — | Avoids Stranski-Krastanov regime |
Key Methodologies
Section titled “Key Methodologies”- Substrate Selection: Use high-quality HPHT Type IIa diamond substrates with minimal pre-existing threading dislocations (< 4 cm-2) to isolate dislocation generation mechanisms intrinsic to the epilayer.
- Epilayer Growth (MPCVD):
- Maintain 2D layer-by-layer growth; avoid Stranski-Krastanov transition.
- Adjust CH4/H2 ratio within 0.15%-4% to tune the Critical Boron Level (CBL).
- Select growth orientation ([100] or [111]) deliberately, as [100] tolerates roughly 3× higher boron concentrations before proximity-induced dislocations occur.
- Doping Control:
- Target [B] below the CBL line (see Table I in paper) for the chosen orientation and CH4/H2 ratio.
- Keep epilayer thickness below the People and Bean critical thickness (hc) to suppress strain-driven misfit dislocation formation.
- Lattice Parameter Mapping: Interpolate the diamond lattice parameter a(x) for boron concentrations up to 2% atomic using linear Vegard-like behavior (Brazhkin et al. data).
- Dislocation Modeling: Compare three critical-thickness models — Matthews-Blakeslee (M-B), People-Bean (P-B), Van der Merwe (V-M) — to determine which mechanism governs under given (thickness, [B], orientation) conditions.
- Defect Characterization:
- Use Dark-Field TEM along [004], [011], [001] zone axes to image dislocations.
- Apply High-Angle Annular Dark-Field (HAADF) STEM for sub-50 nm layers.
- Track dislocation position (top vs. interface) to determine Peach-Koehler force activity.
- Process Window Validation: Confirm that epilayers grown in the dislocation-free region (below CBL line and below P-B hc) yield defect-free layers even at high doping (2 × 1021 cm-3) and thicknesses as low as 10 nm.
6CCVD Solutions & Capabilities
Section titled “6CCVD Solutions & Capabilities”Applicable Materials
Section titled “Applicable Materials”- Heavy Boron-Doped Polycrystalline Diamond (BDD): For cost-sensitive device prototyping where single-crystal substrates are not required, 6CCVD supplies BDD with tunable resistivity to replicate the [B] = 1020-1021 cm-3 regimes studied here.
- Optical Grade Single Crystal Diamond (SCD): For replication of the exact HPHT homoepitaxy experiments described in this paper, 6CCVD provides Type IIa SCD substrates (low TD density) and offers custom epitaxial BDD layers grown on customer-supplied or in-house SCD substrates.
- Custom-Thickness BDD Epilayers: 6CCVD’s SCD/PCD thickness range (0.1 µm - 500 µm) directly covers the 10 nm - 500 nm epilayer window analyzed in this work, enabling clients to fabricate both ultra-thin test structures and full device layers.
Customization Potential
Section titled “Customization Potential”- Orientation-Specific Growth: This paper proves that [100] orientation tolerates roughly 3× higher [B] than [111]. 6CCVD accommodates custom requests specifying (100) or (111) oriented SCD substrates and matched BDD epilayer growth.
- Process Window Tuning: Because CBL scales with the CH4/H2 ratio, 6CCVD offers bespoke MPCVD recipe development to position clients inside the dislocation-free region (below CBL and below P-B hc) for their target doping-thickness combination.
- Wafer Dimensions: Epilayers can be deposited on substrates up to 125 mm (PCD), enabling wafer-scale BDD device fabrication well beyond the small coupons typically used in academic studies.
- Metallization for Device Fabrication: This paper targets diodes and transistors. 6CCVD provides in-house Ti, Pt, Au, Pd, W, and Cu metallization, including the Ti/Pt/Au stacks commonly used for ohmic contacts to p-type BDD. Custom patterning and laser cutting services are available for rapid prototyping of Schottky diodes, MESFETs, and BJT structures.
Engineering Support
Section titled “Engineering Support”- 6CCVD’s in-house PhD engineering team can assist with material selection for high-power, high-frequency, and radiation-hard diamond electronic device projects, including guidance on dislocation-free growth windows, optimal [B] targeting, and substrate/epilayer orientation matching.
- For clients transitioning from single-layer TEM-validation studies (as in this paper) to full multi-layer device stacks, 6CCVD offers consultation on layer stacking, doping gradients, and metallization schemes.
Call to Action
Section titled “Call to Action”For custom specifications or material consultation on heavily boron-doped diamond epilayers, visit 6ccvd.com or contact our engineering team directly. Global shipping available (DDU default; DDP on request).
View Original Abstract
Doping diamond layers for electronic applications has become straightforward during the last two decades. However, dislocation generation in diamond during the microwave plasma enhanced chemical vapor deposition growth process is still not fully understood. This is a truly relevant topic to avoid for an optimal performance of any device, but, usually, it is not considered when designing diamond structures for electronic devices. The incorporation of a dopant, here boron, into a lattice as close as that of diamond, can promote the appearance of dislocations in the epilayer. The present contribution analyzes the different processes that can take place in this epilayer and gives some rules to avoid the formation of dislocations, based on the comparison of the different dislocation generation mechanisms. Indeed, competitive mechanisms, such as doping atom proximity effect and lattice strain relaxation, are here quantified for heavily boron-doped diamond epilayers. The resulting growth condition windows for defect-free heavily doped diamond are here deduced, introducing the diamond parameters and its lattice expansion in several previously published critical thickness (hc) and critical doping level relationships for different doping levels and growth conditions. Experimental evidence supports the previously discussed thickness-doping-growth condition relationships. Layers with and without dislocations reveal that not only the thickness but also other key factors such as growth orientation and growth parameters are important, as dislocations are shown to be generated in epilayers with a thickness below the People and Bean critical thickness.
Tech Support
Section titled “Tech Support”Original Source
Section titled “Original Source”References
Section titled “References”- 2018 - Power Electronic Devices Applications of Diamond Semiconductors