Skip to content

Effects of Cold Spraying Process and Diamond Addition on Microstructure and Thermal Conductivity of Copper Matrix Composites

MetadataDetails
Publication Date2023-01-01
JournalJournal of Physics Conference Series
AuthorsDan Wu, Linwei Zhang, Youliang Zhang, Yanqi Zeng, Qiang Hu
InstitutionsJiangxi Academy of Sciences
AnalysisFull AI Review Included

Cold Spraying of Copper-Diamond Composites for High Thermal Conductivity Packaging

Section titled “Cold Spraying of Copper-Diamond Composites for High Thermal Conductivity Packaging”
  • Application: High-performance electronic packaging requiring both high thermal conductivity (TC) and a tailored coefficient of thermal expansion (CTE) to match semiconductor dies.
  • Reinforcement Strategy: Diamond particles embedded in a copper matrix leverage diamond’s extremely high intrinsic TC while copper supplies ductility and electrical conductivity.
  • Process Used: Cold spraying (CS) — a solid-state kinetic deposition technique using helium carrier gas heated to several hundred degrees Celsius to accelerate Cu and diamond-Cu composite powders above the speed of sound onto a substrate.
  • Interface Engineering: Copper-plated diamond powder is used to overcome the inherently poor wettability and weak Cu/diamond bonding that otherwise limits interfacial heat transfer.
  • Key Findings:
    • Increasing carrier gas temperature slightly reduces the flattening ratio of deformed Cu splats (splats shift from lamellar to more rounded morphology), indicating thermal softening of Cu particles.
    • Cycle count (1 → 3 passes) has negligible impact on microstructure and TC — confirming CS process robustness and reproducibility.
    • TC rises monotonically with carrier gas temperature in the 400 °C - 600 °C range.
    • Adding only 20 vol% diamond is insufficient — TC actually drops vs. pure Cu, indicating that higher diamond loading (>30 vol%) is required to benefit from the diamond reinforcement pathway.
  • Engineering Takeaway: Cold spray is a viable, low-oxygen, high-density route to diamond-Cu composites, but achieving the theoretical thermal performance ceiling requires both proper diamond surface metallization and higher-than-conventional reinforcement volume fractions.
ParameterValueUnitContext
Matrix materialCu (copper powder)—Deforms plastically during CS impact
ReinforcementDiamond particles (Cu-plated)—Surface metallization improves wettability
Carrier gasHelium (He)—Heated working gas for CS acceleration
Carrier gas temperature range400 - 600°CDrives particle velocity and softening
Particle velocitySeveral × speed of soundm·s-1Typical CS regime (supersonic)
Cycle times evaluated1, 2, 3passesSamples labelled Cu-1, Cu-2, Cu-3
Diamond addition tested20vol%Insufficient; caused TC reduction
Recommended diamond loading>20 (ideally 40-60+)vol%Required for TC uplift vs. pure Cu
Diamond particle size~50 - 100µmPer SEM micrographs (Figure 2)
Cu powder morphologySpherical, mixed gel-powder—Feedstock appearance
Splat morphology vs. tempLamellar → near-spherical—Flattening ratio decreases with rising T
Splat morphology vs. cyclesStable across 1-3 passes—High process reproducibility
Measured TC trend (vs. T)Rising from ~275 to ~325W·m-1·K-1 (approx., per Figure 5b)400 °C → 600 °C
Measured TC trend (vs. cycles)Flat / negligible change—Confirms process robustness
Target applicationElectronic packaging—High-power, high-density devices
  1. Feedstock Preparation
    • Spherical Cu powder as the matrix phase.
    • Diamond particles (~50-100 µm) pre-coated with a Cu layer (electroless/electrolytic Cu plating) to suppress the native Cu/diamond interfacial thermal resistance.
    • Mechanical mixing of Cu-plated diamond and Cu powder prior to spraying.
  2. Cold Spray Deposition
    • Helium carrier gas heated to 400 °C, 500 °C, or 600 °C.
    • Gas-particle stream accelerated to several times the speed of sound.
    • Supersonic impact onto substrate → severe plastic deformation of Cu → bonding without melting.
    • Samples produced with 1, 2, or 3 spray cycles to study pass-count effects.
  3. Microstructural Characterization
    • Optical and scanning electron microscopy (SEM) of cross-sections to assess splat morphology, flattening ratio, and diamond distribution at Cu grain boundaries.
    • Energy-dispersive X-ray spectroscopy (EDS) mapping for elemental verification of Cu plating on diamond.
  4. Thermal Conductivity Measurement
    • TC evaluated as a function of three independent variables: cycle number (1-3), carrier gas temperature (400-600 °C), and diamond content (0-20 vol%).
  5. Interpretation
    • Carrier gas temperature → governs particle softening and final splat geometry.
    • Diamond content → governs interfacial phonon/electron transport pathways; low loading (<20%) behaves as defect sites rather than percolating heat conduits.
  • Applicable Materials:
    • For replication or extension of this Cu/diamond heat-spreader research, 6CCVD’s Optical Grade and Thermal Grade Single Crystal Diamond (SCD) — or High-Purity Polycrystalline Diamond (PCD) with grain sizes engineered for phonon transport — can serve as premium feedstock alternatives where monodisperse, narrow-size-fraction, defect-controlled diamond particles are required.
    • Where the paper specifies Cu-plated diamond powder, 6CCCCVD’s Boron-Doped Diamond (BDD) or surface-engineered PCD particles can be supplied with controlled surface chemistry, custom size cuts (50-100 µm or other), and tailored sp2/sp3 ratios to maximize Cu/diamond interface quality and minimize Kapitza resistance.
  • Customization Potential:
    • 6CCVD offers custom dimensions for diamond plates, wafers, and substrates up to 125 mm (PCD), with thickness from 0.1 µm to 500 µm for SCD/PCD and substrates up to 10 mm.
    • For composite feedstock development, 6CCVD can provide custom metalization layers (Ti, Cr, Au, Pt, Pd, W, Cu) on diamond surfaces — directly supporting the Cu-on-diamond plating strategy used in this study. Both electroless-style and PVD-deposited metallization are available in-house.
    • In-house laser cutting and shaping enable precise, narrow PSD (particle size distribution) fractionation of bulk diamond plates if researchers need precisely characterized diamond flake or particle feedstock beyond conventional crushed powders.
    • For downstream device-level packaging, 6CCVD can deliver ultra-low surface roughness diamond (Ra &lt; 1 nm for SCD, &lt; 5 nm for inch-size PCD) suitable for direct die attachment or as heat-spreader inserts.
  • Engineering Support:
    • 6CCVD’s in-house PhD engineering team can collaborate on material selection for thermal-management and high-power electronic packaging projects, including:
      • Diamond particle size distribution optimization for composite percolation thresholds.
      • Surface metalization stack selection (e.g., Ti/Pt/Au vs. direct Cu) for Cu/diamond interface engineering.
      • Trade-off analysis between SCD, PCD, and BDD particles as a function of composite thermal performance targets and cost constraints.
    • Whether the research goal is scaling up diamond volume fraction (>30 vol%), transitioning from cold spray to SPS (spark plasma sintering) or hot pressing, or qualifying diamond for high-power LED, GaN, or SiC die attach, 6CCVD can support prototype-to-pilot material supply.
  • Call to Action: For custom specifications, metalization stacks, or material consultation on diamond-reinforced metal matrix composites, visit 6ccvd.com or contact our engineering team directly.
View Original Abstract

Abstract The operation speed and integration degree of electronic components are getting higher and higher, which puts forward higher requirements for electronic packaging materials. Diamond is added to copper matrix composites to improve the thermal conductivity. The effects of cold spraying process and diamond addition on the microstructure and thermal conductivity of copper matrix composites are studied. The results show that the copper matrix composite prepared by cold spraying is a deformed strip copper layer. The change of cycle times has little effect on the microstructure, while the flattening rate of the deformed copper layer decreases as the carrier gas temperature increases. The diamond particles are uniformly distributed at the copper grain boundary after adding copper plated diamond powder, which are closely bound to the copper matrix. Increasing the temperature is conducive to increasing the thermal conductivity, while the change of cycle times has little effect on it. The addition of 20% diamond particles reduces the thermal conductivity, so the diamond content should be increased to play its role in thermal conductivity.