Polycrystalline Diamond Micro‐Hotplates
At a Glance
Section titled “At a Glance”| Metadata | Details |
|---|---|
| Publication Date | 2023-08-02 |
| Journal | Small |
| Authors | Evan L. H. Thomas, Jaspa Stritt, Soumen Mandal, Matthias Imboden, Oliver A. Williams |
| Institutions | Cardiff University |
| Citations | 5 |
| Analysis | Full AI Review Included |
Executive Summary
Section titled “Executive Summary”- Material Innovation: Successful fabrication of freestanding micro-hotplates from a single layer of heavily boron-doped polycrystalline diamond (BDD/PCD), eliminating multi-layer CTE mismatch and electro-migration failures.
- Extreme Operating Temperatures: Achieved peak temperatures of 2731 K at ≤ 100 mW applied power, vastly surpassing the ~1600 K limit of conventional poly-Si or Pt hotplates.
- Grey-Body Emission: Exhibits constant emissivity (~0.63) across 475-1700 nm, driven by boron-acceptor absorption and surface-roughness scattering—ideal for IR sources and FTIR applications.
- Rapid Thermal Response: Millisecond-scale thermalization times, an order of magnitude faster than membrane structures limited to 1600 K.
- Geometry-Driven Performance: Octagonal and square geometries with serpentine spring-like tethers mitigate buckling and allow joule heating via constrictive 3 µm wide supporting arms.
- Failure Mechanism Insight: Raman spectroscopy confirms that performance limits beyond 1349 K are dictated by cumulative graphitization to sp2 carbon, with lifetimes extending to > 7 days at ~5 mW (low-power operation).
- Application Scope: Validated for broadband IR sources, NDIR gas sensors, and in-situ UHV heater stages for high-resolution electron microscopy.
Technical Specifications
Section titled “Technical Specifications”| Parameter | Value | Unit | Context |
|---|---|---|---|
| Material | Heavily boron-doped PCD | — | Single-layer freestanding element |
| Diamond film thickness | ~1.5 | µm | Conformal CVD over substrate |
| Boron concentration | > 1021 | cm-3 | Above metallic-like transport threshold |
| Resistivity regime | Metallic-like | — | B/C feed gas ratio tuned for conductivity |
| Average grain size | ~500 | nm | Van der Drift competitive overgrowth morphology |
| Through-hole diameter | 3 | µm | Sacrificial etch access |
| Arm width | 3 | µm | Constrictive serpentine tethers |
| Arm lengths tested | 30, 80 | µm | Octagonal hotplate variants |
| Peak temperature achieved | 2731 | K | Maximum reported, large octagonal hotplate |
| Temperature (4 min bias hold) | ~1800 | K | Plateau region |
| Temperature (10 sec bias hold) | 2213-2339 | K | Small/large octagonal |
| Temperature (square hotplates) | 2000-2200 | K | Steady-state upper limit |
| Onset of InGaAs detection | ~600 | K | Near-IR emission threshold |
| Applied power (peak) | ≤ 100 | mW | Includes ~55 mW (small) / ~110 mW (large) plateau |
| Applied power (square devices) | ~5-20 | mW | Bias-dependent lifetime tests |
| Operating voltage range | 1.0-6.5 | V | Increments of 0.25 V |
| Bias hold durations | 10 sec, 1 min, 4 min | — | Thermal stress vs. lifetime trade-off |
| Emissivity | 0.63 | — | Grey-body approximation for similar BDD films |
| Emission spectral range | 475-1700 | nm | Si + InGaAs detector coverage |
| Thermalization time | ~millisecond | ms | Faster than conventional membrane hotplates |
| Lifetime at ~5 mW | > 7 | days | Power deviation < 0.5% |
| Lifetime at 10-20 mW | ~1 | hour | Higher operating temperature regime |
| Vacuum test pressure | ≤ 5 × 10-4 | mbar | High-vacuum environment |
| Bond-pad metalization | Cr/Au | — | Bilayer for wire-bonding and low contact resistance |
Key Methodologies
Section titled “Key Methodologies”- Substrate Preparation: Bosch etching of a 12 × 12 mm silicon-on-insulator (SOI) wafer to define the freestanding membrane geometry and underlying sacrificial silicon.
- Seeding & Growth: Uniform nano-diamond seeding followed by conformal MPCVD of a ~1.5 µm thick heavily boron-doped diamond film under high power density, low methane conditions yielding ~500 nm lateral grain size.
- Patterning: Standard micro-fabrication (lithography + etching) to define octagonal/square radiator elements, 3 µm through-holes, and serpentine supporting arms.
- Release: Backside sacrificial silicon etch through the 3 µm through-holes to create the freestanding structure.
- Contact Formation: Deposition of Cr/Au bilayer at anchor trenches for low-resistance bond-pad contacts and reliable wire-bonding.
- Packaging: Individual dies mounted and wire-bonded in 16-pin open-top DIP packages.
- Electrical Characterization: Keithley 2450-EC source measure unit for I-V sweeps and steady-state biasing with incremental voltage steps.
- Thermal Characterization (Raman): Horiba LabRAM HR Evolution with 473 nm excitation, 50x objective, 600 grmm-1 grating; laser blanked to capture thermal emission spectrum.
- Thermal Characterization (Monochromator): Bentham TMS300 with DH_Si (500-1100 nm) and DH_IGA (up to 1700 nm) detectors; calibrated against Oriel 63358 45 W quartz tungsten halogen lamp.
- Transient Response: 20 Hz square-wave excitation (GW Instek AFG-2005), 1 Ω shunt resistor with INA293 current sense amplifier, Agilent DSO7014A oscilloscope.
- Raman Spectroscopy (Post-Test): Tracking D (~1350 cm-1) and G (~1595 cm-1) peak emergence to characterize graphitization onset at > 1349 K.
6CCVD Solutions & Capabilities
Section titled “6CCVD Solutions & Capabilities”-
Applicable Materials:
- This research relies on Heavy Boron-Doped Polycrystalline Diamond (BDD/PCD) with boron concentrations exceeding 1021 cm-3 to achieve metallic-like transport and high emissivity (~0.63).
- 6CCVD supplies freestanding BDD/PCD membranes and thin-film BDD coatings grown via MPCVD, with thicknesses spanning 0.1 µm to 500 µm for PCD layers—well aligned with the ~1.5 µm thickness used here.
- For applications requiring higher emissivity tuning or alternative morphologies, Optical Grade SCD (Ra < 1 nm) and standard polycrystalline substrates are also available.
-
Customization Potential:
- The paper employs Cr/Au metalization at the bond-pads and serpentine 3 µm arm geometries. 6CCVD offers in-house metalization (Au, Pt, Pd, Ti, W, Cu) with custom patterning and laser cutting services to replicate or refine these layouts.
- Custom plate dimensions up to 125 mm (PCD) allow direct fabrication of large-area wafers for wafer-scale MEMS processing.
- Substrate thicknesses can be specified up to 10 mm for robust handling during Bosch etching and backside release steps.
- Through-hole patterning, serpentine arm definition, and membrane release windows can be supported through custom lithography-ready wafers.
-
Engineering Support:
- 6CCVD’s in-house PhD team can assist with material selection for next-generation micro-hotplate, IR source, and NDIR gas sensor projects.
- Expertise available for optimizing boron-doping levels to balance conductivity, emissivity, and graphitization threshold for your specific operating temperature window.
- Consultation on surface roughness (Ra < 5 nm for inch-size PCD) to fine-tune grey-body emission characteristics or reduce optical interference effects in your device stack.
-
Call to Action: For custom specifications, BDD membrane fabrication, or material consultation tailored to high-temperature MEMS and IR emitter applications, visit 6ccvd.com or contact our engineering team directly.
View Original Abstract
Abstract Micro‐hotplate structures are increasingly being investigated for use in a host of applications ranging from broadband infra‐red sources within absorption‐based gas sensors to in situ heater stages for ultra‐high‐resolution imaging. With devices usually fabricated from a conductive electrode placed on top of a freestanding radiator element, coefficient of thermal expansion (CTE) mismatches between layers and electro‐migration within the heating element typically lead to failure upon exceeding temperatures of 1600 K. In an attempt to mitigate such issues, a series of hotplates of varying geometry have been fabricated from a single layer of mechanically robust, high thermal conductivity, and low CTE boron‐doped polycrystalline diamond. Upon testing under high vacuum conditions and characterization of the emission spectra, the resulting devices are shown to exhibit a grey‐body like emission response and reach temperatures vastly in excess of conventional geometries of up to 2731 K at applied powers of ⩽100 mW. Characterization of the thermalization time meanwhile demonstrates rapid millisecond response times, while Raman spectroscopy reveals the performance of the devices is dictated by cumulative graphitization at elevated temperatures. As such, both diamond and sp 2 carbon are shown to be promising materials for the fabrication of next‐generation micro‐hotplates.