Structural and Functional Properties of Si and Related Semiconducting Materials Processed by High-Pressure Torsion
At a Glance
Section titled “At a Glance”| Metadata | Details |
|---|---|
| Publication Date | 2024-07-25 |
| Journal | Journal of the Japan Institute of Metals and Materials |
| Authors | Yoshifumi Ikoma |
| Institutions | Materials Science & Engineering, Kyushu University |
| Analysis | Full AI Review Included |
Structural and Functional Properties of Si and Related Semiconducting Materials Processed by High-Pressure Torsion
Section titled “Structural and Functional Properties of Si and Related Semiconducting Materials Processed by High-Pressure Torsion”Executive Summary
Section titled “Executive Summary”- Novel Phase Engineering: Demonstrates high-pressure torsion (HPT) processing at 6 GPa to induce strain-driven phase transformations in Si, yielding metastable phases (Si-III, Si-XII, Si-IV) that are unattainable under ambient conditions.
- Semimetallic Behavior: Confirms the formation of semimetallic bc8-Si0.5Ge0.5 from SiGe alloys, opening pathways for narrow-bandgap semiconductor devices.
- Thermal Conductivity Suppression: Achieves a dramatic reduction in Si thermal conductivity from ~140 W m-1 K-1 to ~3 W m-1 K-1 through grain refinement and metastable phase formation.
- Electrical Transport Modulation: Documents resistivity decrease from ~0.2 Ω m to ~7 × 10-3 Ω m with increasing anvil rotations (N), driven by the formation of semimetallic Si-III.
- Optical Properties: Reports broad, weak photoluminescence (PL) in the visible region after 873 K annealing, attributed to quantum confinement in Si-I nanograins.
- Scale-Up Potential: HPT enables millimeter-to-centimeter-scale bulk sample preparation, unlike traditional diamond anvil cell (DAC) methods limited to microscopic volumes.
- Material Versatility: Explores both Si and Si0.5Ge0.5 alloys, with implications for photovoltaics, thermoelectrics, and quantum-confined optoelectronics.
Technical Specifications
Section titled “Technical Specifications”| Parameter | Value | Unit | Context |
|---|---|---|---|
| Nominal HPT Pressure (Si) | 6 | GPa | Low-pressure phase transformation regime |
| Nominal HPT Pressure (SiGe) | 24 | GPa | High-pressure alloy processing |
| Anvil Rotation Speed | 1 | rpm | Constant for all experiments |
| Anvil Rotations (N) | 10, 50, 100 | turns | Variable strain parameter |
| Sample Diameter (Si) | 5-10 | mm | Disk geometry |
| Sample Diameter (SiGe) | 5 | mm | Disk geometry |
| Sample Thickness | 0.25 | mm | Tungsten carbide anvil depth |
| Bulk Si Thermal Conductivity | ~140 | W m-1 K-1 | Reference single-crystal value |
| HPT Si Thermal Conductivity (N=10) | ~10 | W m-1 K-1 | After HPT processing |
| HPT Si Thermal Conductivity (N≥50) | ~3 | W m-1 K-1 | Saturation at high rotations |
| Si-III Theoretical Thermal Conductivity | 4 | W m-1 K-1 | DFT calculation at 300 K |
| Si-XII Theoretical Thermal Conductivity | 19 | W m-1 K-1 | DFT calculation at 300 K |
| Si Initial Resistivity (N=10) | ~0.2 | Ω m | After minimal HPT |
| Si Resistivity (N=50) | ~2 × 10-2 | Ω m | Mid-range HPT |
| Si Resistivity (N=100) | ~7 × 10-3 | Ω m | Maximum reduction |
| Si0.5Ge0.5 Resistivity (As-grown) | ~9 × 10-5 | Ω m | TLZ-grown crystal baseline |
| Si0.5Ge0.5 Resistivity (N=0) | ~5 × 10-4 | Ω m | After compression only |
| Si-I Bandgap | 1.12 | eV | Indirect, diamond-cubic phase |
| Si-III Bandgap | 30 | meV | Semimetallic bc8 phase |
| Si-IV Bandgap | 0.95 | eV | Indirect, hexagonal diamond (lonsdaleite) |
| Si-XII Bandgap | 0.24 | eV | r8 rhombohedral phase |
| Si-II Transformation Pressure | ~11 | GPa | Diamond-cubic to β-Sn (static) |
| HPT-Induced Transformation Pressure | <11 | GPa | Shear-assisted, lower threshold |
| Si0.5Ge0.5 Lattice Parameter (bc8) | 0.678 | nm | Vegard’s law value: 0.6784 nm |
| Si-III Lattice Parameter | 0.6636 | nm | bc8 reference |
| Ge-IV Lattice Parameter | 0.6932 | nm | bc8 reference |
| Grain Size (Si, N=10) | ~10 | nm | Order of magnitude |
| Grain Size (Si, N≥50) | <10 | nm | Si-I, Si-III, and Si-XII |
| Si-I Volume Fraction (N=100) | ~0.5 | — | Remaining diamond-cubic phase |
| Si-III Volume Fraction (N=100) | >0.3 | — | Semimetallic bc8 phase |
| Si-XII Volume Fraction (N=100) | ~0.2 | — | r8 phase saturation |
| Annealing Temperature (Si-IV Formation) | 433-473 | K | Phase transition window |
| Ex-situ Annealing Conditions | 473 K, 2 h, N2 | — | Si-III to Si-IV conversion |
| PL Excitation Wavelength | 488 | nm | Room temperature measurement |
| PL Annealing Temperature | 873 | K | 1 h in N2 atmosphere |
| Specific Heat Capacity (Reference) | 0.71 | J g-1 K-1 | Used for thermal conductivity calculation |
| Synchrotron X-ray Energy | 61.4 | keV | SPring-8 BL04B1 beamline |
| XRD Source (Lab) | Cu Kα | — | Standard laboratory characterization |
Key Methodologies
Section titled “Key Methodologies”- Substrate Preparation: Single-crystal Si(100) wafers and traveling-liquidus-zone (TLZ)-grown Si0.5Ge0.5 bulk crystals cut into 5 mm or 10 mm diameter disks with 0.25 mm thickness.
- HPT Processing: Samples set into tungsten carbide (WC) anvils with 0.25 mm cavities; processed at room temperature under nominal pressures of 6 GPa (Si) or 24 GPa (SiGe) at 1 rpm rotation.
- Variable Strain Control: Anvil rotation number (N) varied at 10, 50, and 100 turns to modulate shear strain (γ = 2πrN/t) and track phase evolution.
- In-Situ Synchrotron XRD: High-energy X-ray diffraction performed at SPring-8 BL04B1 (photon energy 61.4 keV) during annealing up to 473 K to observe real-time phase transitions.
- Ex-Situ Annealing: HPT-processed Si samples annealed at 473 K for 2 h in N2 atmosphere to confirm Si-IV (lonsdaleite) formation.
- Microstructural Characterization: High-resolution transmission electron microscopy (HRTEM) with FFT analysis for nanograin identification and phase confirmation.
- Ex-Situ XRD: Cu Kα laboratory XRD for post-processing phase identification and Rietveld refinement of volume fractions.
- Resistivity Measurements: Four-probe method with 1 mm probe spacing for electrical transport characterization.
- Thermal Conductivity Calculation: κ = αcρ, where α is thermal diffusivity (laser flash method), c is specific heat (0.71 J g-1 K-1), and ρ is density (calculated from Si-I, Si-III, Si-XII volume fractions).
- Photoluminescence Spectroscopy: Room-temperature PL using 488 nm laser excitation to detect quantum confinement in Si-I nanograins after 873 K annealing.
6CCVD Solutions & Capabilities
Section titled “6CCVD Solutions & Capabilities”The presented research on phase transformation, nanostructuring, and metastable phase engineering in semiconductors aligns directly with several high-performance material categories available through our manufacturing capabilities.
Applicable Materials
Section titled “Applicable Materials”- Optical Grade Single Crystal Diamond (SCD): For research groups requiring diamond anvil cell (DAC) alternatives or high-pressure environments exceeding the 6 GPa threshold demonstrated here, our SCD substrates (up to 10 mm thickness) with Ra < 1 nm polishing provide an ideal optical window and gasket material for optical/Raman spectroscopy under extreme pressure.
- Polycrystalline Diamond (PCD) Plates: For large-area applications requiring uniform mechanical robustness, our PCD plates up to 125 mm diameter serve as robust anvils or wear-resistant components in high-pressure tooling and SPD (severe plastic deformation) apparatus.
- Boron-Doped Diamond (BDD): For electrical transport studies or electrode applications in electrochemical environments, our BDD offers tunable resistivity from semimetallic to insulating regimes, paralleling the semiconductor-to-semimetal transition demonstrated in HPT-processed Si.
Customization Potential
Section titled “Customization Potential”- Custom Wafer Dimensions: The paper utilizes 5 mm and 10 mm Si disks. For replication or extended research, 6CCVD can provide laser-cut diamond wafers and substrates in custom dimensions with tight tolerances, enabling integration with HPT fixtures or specialized sample holders.
- Metalization Services: For electrical contact preparation on HPT-processed samples (critical for four-probe resistivity measurements), we offer in-house metalization with Ti, Pt, Au, Pd, W, and Cu. A Ti/Pt/Au stack is particularly suitable for stable Ohmic contacts on Si and SiGe alloys across broad temperature ranges.
- Precision Polishing: Our Ra < 1 nm (SCD) and < 5 nm (PCD) surface finishes ensure minimal surface scattering effects in optical or electrical characterization, critical for accurate PL and resistivity measurements on nanostructured semiconductors.
Engineering Support
Section titled “Engineering Support”- Material Selection Consultation: 6CCVD’s in-house PhD engineering team can assist with material selection for high-pressure research, optical window design, and electrode integration in semiconductor phase transformation studies.
- Prototype Development: For researchers extending this work to diamond-Si hybrid structures or diamond-protected semiconductor devices, we can support rapid prototyping of custom diamond components with metalized contacts and laser-cut geometries.
- Application Areas: Photovoltaics, thermoelectric devices, quantum-confined optoelectronics, narrow-bandgap semiconductor devices, and metastable phase exploitation.
Call to Action
Section titled “Call to Action”For custom specifications or material consultation, visit 6ccvd.com or contact our engineering team directly.
View Original Abstract
We report on high-pressure torsion (HPT) processing of Si and related semiconducting materials, and discuss their phase transformations and electrical, thermal, and optical properties. In-situ synchrotron x-ray diffraction revealed that the metastable bc8-structure Si-III and r8-structure Si-XII in the HPT-processed Si samples gradually disappeared and hexagonal-diamond Si-IV appeared during annealing up to 473 K. The formation of Si-III/XII in the samples processed at a nominal pressure of 6 GPa indicated the strain-induced phase transformation from diamond-cubic Si-I to a high-pressure tetragonal Si-II phase during HPT processing, and a following phase transformation from Si-II to Si-III/XII upon decompression. The resistivity decreased with increasing the number of anvil rotations due to the formation of semimetallic Si-III. The thermal conductivity of Si was reduced to ∼3 Wm−1K−1 after HPT processing. A weak and broad photoluminescence peak associated with Si-I nanograins appeared in the visible light region after annealing. Metastable bc8-Si0.5Ge0.5 with a semimetallic property was formed by HPT processing of a traveling-liquidus-zone-grown Si0.5Ge0.5 crystal. These results indicate that the application of HPT processing to Si and related semiconductors paves the way to novel devices utilizing nanograins and metastable phases.