Scratching of Diamond Substrate Using Fixed Ultra-Hard Abrasive Grain Tool
At a Glance
Section titled “At a Glance”| Metadata | Details |
|---|---|
| Publication Date | 2026-01-01 |
| Journal | International Journal of the Society of Materials Engineering for Resources |
| Authors | Hiroyuki MIZUMA, Masanobu Nakatsu, Tatsuya MIYOTA, Kota NAGAO, Ryota NAMIKI |
| Institutions | Nikon (Japan), Akita University |
| Analysis | Full AI Review Included |
Executive Summary
Section titled “Executive Summary”- Core Challenge: Machining single-crystal diamond (SCD) substrates is notoriously difficult due to diamond’s extreme hardness and chemical inertness. Traditional polishing is extremely slow (cutting depth < 1 µm/km).
- Material Investigation: Four ultra-hard candidates were evaluated as abrasive grains fixed to a wheel saw: Fullerene (C60), Wurtzite Boron Nitride (w-BN), Polycrystalline Diamond (PCD), and Flame Combustion-Synthesized Diamond (FCSD).
- Key Finding — Grain Geometry Matters: Hardness alone is insufficient. Grain morphology (sharpness and size ≥ 8 µm) and fracture toughness dictate performance. Fullerene and w-BN crushed too easily (van der Waals bonding); PCD grains were too smooth.
- Winning Abrasive: Flame Combustion-Synthesized Diamond (FCSD) was identified as the most promising abrasive. Its irregular, angular shape effectively initiates micro-cleavage fractures along the diamond’s (111) planes.
- Operational Threshold: The transition from polishing to scratching requires a minimum load of ~2.7 N (275 gf), producing scratch widths of approximately 8 µm.
- Strategic Implication: Future manufacturing requires saw wires equipped with FCSD grains to enable controlled brittle-fracture cutting rather than slow friction-based polishing.
Technical Specifications
Section titled “Technical Specifications”| Parameter | Value | Unit | Context |
|---|---|---|---|
| Diamond Substrate Size | 4 × 4 × 0.5 | mm | SCD workpiece dimensions |
| Wheel Saw Dimensions | φ16 × 0.5 | mm | Fixed-grain cutting tool |
| Cutting Load (Wheel Saw) | ~3 | N | Applied normal force during cutting |
| Circumferential Speed | ~80 | m/min | Wheel saw rotational velocity |
| Polishing Speed | < 1 | µm/km | (Cutting depth / traveling distance) |
| Scratch Threshold Load | ≥ 2.7 (275 gf) | N | Transition from polish to scratch |
| Scratch Width | ~8 | µm | Average scratch width at 2.7 N |
| PCD Grain Size | 4 - 8 | µm | Summitt Super Abrasive Co. |
| w-BN Max Grain Size | 10 | µm | Goodfellow Cambridge |
| Fullerene Composition | 99% C60 / 1% C70 | — | Frontier Carbon “Nanom Purple ST” |
| FCSD Film Thickness | ~20 | µm | As-synthesized film before crushing |
| FCSD Crushed Grain Size | < 20 | µm | Post-crushing in crucible |
| Brazing Alloy | Cu 85 / Sn 15 | wt% | Bronze brazing filler |
| Reducing Agent | TiH2 | — | Generates reducing atmosphere in vacuum furnace |
| Cleavage Plane Exploited | (111) | — | Secondary cracks indicate brittle fracture along this plane |
| Substrate Orientation | (100) | — | Workpiece crystal face |
Key Methodologies
Section titled “Key Methodologies”- Material Selection: Four ultra-hard grain candidates (Fullerene, w-BN, PCD, FCSD) containing elements with consecutive atomic numbers (B, C, N) were selected.
- Grain Fixation: Abrasive grains were brazed onto a steel wheel saw substrate using a Cu-Sn (85/15) bronze alloy in a high-temperature, high-vacuum furnace.
- Atmosphere Control: TiH2 was added to the brazing setup to decompose and generate a reducing atmosphere, overcoming the poor wettability between ceramics and the brazing material.
- Wheel Saw Machining: A φ16 × 0.5 mm rotating wheel saw was applied to a 4 × 4 × 0.5 mm SCD plate under ~3 N load at ~80 m/min circumferential speed.
- Grinding (Fracture Toughness) Test: Grains were sandwiched between two diamond plates and subjected to compressive forces from 0 to 4 N to assess fracture behavior.
- Single-Tip Scratching Test: An indenter with variable load (0-3 N) was used to identify the critical load threshold separating polishing from scratching regimes.
- Surface Analysis: Post-machining SCD surfaces were examined optically to identify scratch morphology, width, and secondary crack propagation along (111) cleavage planes.
6CCVD Solutions & Capabilities
Section titled “6CCVD Solutions & Capabilities”-
Applicable Materials:
- For replicating the workpiece in this study, our Optical Grade Single Crystal Diamond (SCD) plates are ideal. We supply SCD in custom dimensions up to 125 mm (PCD) with thicknesses from 0.1 µm to 500 µm, and substrates up to 10 mm thick for structural/mechanical test coupons.
- For replicating the abrasive grain source, 6CCVD manufactures high-purity Polycrystalline Diamond (PCD) via MPCVD with controlled grain structures — directly applicable for tool insert fabrication when fine, uniform grain sizes are required.
- For applications requiring electrical conductivity during scratching/EDM combined machining, our Heavy Boron-Doped Diamond (BDD) provides tunable resistivity while maintaining extreme hardness.
-
Customization Potential:
- This paper relies on highly specific abrasive grains and brazed tool geometries. 6CCVD supports full-stack customization: we can deliver diamond materials pre-shaped or laser-cut to your tool substrate specifications.
- Our in-house metallization capabilities (Au, Pt, Pd, Ti, W, Cu) enable us to apply custom adhesion layers (e.g., Ti bonding layers) directly to diamond surfaces, facilitating integration into brazed or soldered tool assemblies like the Cu-Sn/TiH2 system described in the paper.
- Surface finishing is controlled to Ra < 1 nm (SCD) and < 5 nm (inch-size PCD), ensuring reference-grade workpiece quality for controlled abrasion experiments.
-
Engineering Support:
- 6CCVD’s in-house PhD engineering team can assist with material selection, crystal orientation optimization (e.g., (100) vs. (111) surface preparation), and grain-size matching for your specific diamond machining or ultra-hard tooling research. Whether you are developing next-generation saw wires, dicing blades, or scratch-testing protocols, our team provides consultative support from prototype to scale.
-
Call to Action:
- For custom specifications, metallization consultation, or material selection for your diamond machining R&D, visit 6ccvd.com or contact our engineering team directly.
View Original Abstract
Scratching tests of a diamond substrate were performed using a tool fixed with four types of grains potentially harder than diamond. Materials reported by other researchers to be harder than diamonds often contain combinations of carbon, boron, and nitrogen. From the viewpoint of manufacturing, fullerene, wurtzite (hexagonal lattice boron nitride), polycrystalline diamond, and flame-synthesized diamond were selected in this study. After creating and testing saw wires and wheel saws, flame combustion synthetic diamond was determined to be the most promising. This is because only scratches from flame combustionsynthesized diamond initiate cleavage fracture.