Skip to content

Thiourea modification of fluorescent nanodiamonds towards enhanced quantum sensing

FieldValue
JournalCarbon Trends
Published2026-01-24
AuthorsPéter Rózsa, Olga Krafcsik, Sándor Lenk, Dávid Beke, Ádám Gali
DOI10.1016/j.cartre.2026.100618
Citations1

Thiourea treatment increased the negatively charged nitrogen-vacancy fraction in 20 nm fluorescent nanodiamonds from 46% to 80%. The paper reports a 72% relative increase under 532 nm excitation at 36 µW.

Nanodiamond NV centers can occupy neutral NV⁰ or negative NV⁻ charge states. The NV⁻ state is most relevant to the quantum applications discussed in the paper. In nanodiamonds, shallow NV centers can lose their extra electron because of surface reactions. Surface states can supply holes under illumination or shift the Fermi level. Adsorbed electrolyte species and fluctuating surface dipoles also aggravate charge instability. These pathways can deplete electrons from shallow NV⁻ centers.

The 20 nm sample therefore provided the strongest test of whether surface chemistry could restore electron availability. Surface termination also affects local band bending and near-surface Fermi-level pinning. Those electronic effects determine the relative populations of NV⁰ and NV⁻. Surface engineering can therefore improve the charge-state population needed for sensing.

The starting material was HPHT fluorescent nanodiamond powder from Adamas Nanotechnology with high NV-center concentrations. The size series covered nominal diameters of 20, 30, 40, 50, 100, and 140 nm.

First, 1 mL of a 1 mg/mL dispersion was diluted to 10 mL and adjusted to pH 14 with ammonia. The authors added 80 mg NaBH₄ and stirred at 70 °C for 12 h to reduce carboxyl groups. The resulting hydroxyl-terminated particles were labeled ND-OH.

Dried ND-OH was redispersed in 3 mL of HBr and HOAc at a 1:2 volume ratio. The authors added 0.11 g thiourea and ultrasonicated the suspension at 80 °C for 3 h. Six millilitres of ice-cooled 7.5 M NaOH was then added to the hot mixture. The reaction continued for 12 h at room temperature.

Concentrated H₂SO₄ adjusted the dispersion to pH 1 to 2. A 1 kDa centrifugal filter purified the product until permeate conductivity reached 0 µS. The resulting thiol-modified particles were labeled ND-SH.

The reaction produced more than isolated thiol groups. FTIR of 20 nm particles showed lower C=O and COOH band intensities after modification. The dominant OH contribution was attributed to the modified surface rather than adsorbed water. The authors expected adsorbed water to contribute only weakly under the 3 mbar FTIR conditions.

Bands broadened from 1000 to 1200 cm⁻¹ and from 1250 to 1550 cm⁻¹. These regions are consistent with C-N, C=N, and sp² carbon vibrations. Expected S-H, C-S, and S-S modes were too weak and obscured for detection.

XPS used monochromatic Al Kα radiation, a 650 µm analysis area, and a base pressure of 3 × 10⁻¹⁰ mbar. The XPS atomic concentrations changed as follows.

SampleC, atomic %N, atomic %O, atomic %S, atomic %
ND20-COOH64.70.834.5Not detected
ND20-SH56.23.837.13.0

Nitrogen components at 399.0 and 400.7 eV represented 61% and 39% of the fitted N 1s signal. The lower-energy component was assigned to pyridinic or imide-like nitrogen. The higher-energy component was assigned to graphitic or quaternary nitrogen.

Sulfur at 167.6 eV represented 93.5% of the fitted S 2p3/2 intensity and was assigned to oxidized sulfur. The 162.9 eV component represented 6.5% and was assigned to thiol or sulfide-like sulfur. The O-C=O component largely disappeared, while a new S=O contribution appeared near 530.6 eV.

Raman spectra at 785 nm retained the diamond peak at 1331 cm⁻¹ and showed no extensive graphitic overlayer. The reported ID/IG ratios were 0.24 for ND-COOH and 0.29 for ND-SH. Under 325 nm excitation, the G band increased for ND-SH. The authors assigned this response to short sp² carbon and nitrogen-rich conjugated fragments. They interpreted the combined results as evidence for conjugated segments rather than extended graphitic layers.

The study did not directly measure the surface Fermi level or charge-transfer kinetics. The authors attribute the larger NV⁻ population to surface thiol and oxygen groups together with nitrogen-rich conjugated byproducts. They propose that this mixture introduces electron-donating and n-type character near the surface. This could raise the local Fermi level and shift the NV⁰/NV⁻ equilibrium toward NV⁻.

The paper therefore treats the result as surface electronic engineering rather than simple thiol attachment. Earlier theoretical work cited by the authors predicted an unfavorable effect from thiol groups. The authors distinguish their outcome from uniform thiol termination, which they describe as potentially destabilizing for shallow NV⁻ centers. The observed gain is attributed to the mixed product chemistry, not to -SH groups alone. That explanation fits the spectroscopy, but it remains a proposed mechanism.

Charge-state results across the size series

Section titled “Charge-state results across the size series”

PL spectroscopy measured NV charge populations before and after treatment. Samples were drop-cast onto polished silicon, and each reported spectrum averaged at least seven positions. Excitation used 532 nm at approximately 36 µW to avoid charge-state conversion. Each spectrum was fitted as a linear combination of pure NV⁰ and NV⁻ spectra by the Levenberg-Marquardt algorithm. The spectra resolved zero-phonon lines at 575 nm for NV⁰ and 637 nm for NV⁻. NV⁻ vibrational bands appeared at 662 and 680 nm.

Nominal sizeND-COOH, mean (SD), %ND-SH, mean (SD), %Relative increase
20 nm46 (1.5)80 (2.3)72%
30 nm59 (4.3)67 (5.3)13%
40 nm65 (2.0)69 (3.3)5%
50 nm67 (3.5)73 (9.4)9%
100 nm76 (5.7)79 (4.8)4%
140 nm72 (7.7)81 (5.6)12%

Relative increases ranged from 4% to 72% across the tested sizes. Other reported increases were 13% at 30 nm, 5% at 40 nm, 9% at 50 nm, and 12% at 140 nm. Treated 20 nm particles reached 80%, nearly matching treated 140 nm particles at 81%. Untreated 20 nm particles were at 46%, compared with 72% for untreated 140 nm particles. The largest standard deviation was 9.4 percentage points for the modified 50 nm sample. Repeated PL measurements after 1 month, 2 months, and 1 year showed no significant change.

Zeta potential measurements used approximately 10⁻³ mg/mL dispersions at 23 °C. Each sample had at least five replicates. After modification, zeta potential became less negative for every tested size. The 100 nm sample shifted from -33.2 mV to -12.5 mV, while the 20 nm sample shifted from -31.5 mV to -20.2 mV. All modified particles retained negative zeta potentials under the measurement conditions.

This supports colloidal dispersibility, but the paper does not report sedimentation, aggregation, or storage tests. FTIR, XPS, and Raman focused on 20 nm particles, while PL and zeta potential covered the full size series. PL spectra were collected from aggregated, drop-cast particles on silicon. The reported fractions are ensemble averages under the stated preparation and measurement conditions.

The study did not report ODMR contrast, spin coherence, magnetic sensitivity, temperature sensitivity, or complete device performance. Thiol conjugation to biomolecules, polymers, and inorganic interfaces was proposed but not demonstrated. Surface chemical characterization was not repeated during the one-year PL stability check.

Surface chemistry should be treated as a design variable for nanodiamonds with near-surface NV centers. For 20 nm particles, thiourea treatment removed the observed size disadvantage in the control series. The measured 80% NV⁻ fraction was obtained with 36 µW excitation and showed no change at the reported one-year remeasurement.

Thiourea treatment also leaves sulfur and nitrogen groups that could support later biomolecule, polymer, or inorganic interface conjugation. Device developers should verify charge-state fraction and zeta potential for each particle size and surface recipe. A higher NV⁻ fraction alone does not establish better thermometry or magnetometry performance. Those metrics still require measurement under the intended sensing conditions.

View Original Abstract

We functionalized fluorescent nanodiamonds of various sizes using a thiourea-based thiolation reaction to tailor their surface chemistry for biological and quantum technological applications. Spectroscopic analyses revealed that this reaction generates a complex mixture of sulfur- and nitrogen-containing groups, arising from the reaction of thiourea with surface functional groups and from oxidative cyclization. Since the charge stability of negatively charged nitrogen-vacancy (NV⁻) centers is strongly influenced by the near-surface electronic structure, surface modifications that enhance this stability—while preserving colloidal dispersibility and enabling further functionalization—are essential for quantum sensing applications. We show that the surface chemistry produced through the reaction of nanodiamonds with thiourea increases electron availability and favors the stabilization of the NV⁻ charge state. These results highlight the potential of thiourea-derived surface modification as an effective route to improve the quantum performance of nanodiamonds.

  1. 2011 - The exocytosis of fluorescent nanodiamond and its use as a long-term cell tracker [Crossref]
  2. 2012 - The long-term stability and biocompatibility of fluorescent nanodiamond as an in vivo contrast agent [Crossref]
  3. 2005 - Bright fluorescent nanodiamonds: No photobleaching and low cytotoxicity [Crossref]
  4. 2023 - Study of fluorescent nanodiamonds concentrations in aqueous solutions for biological applications [Crossref]
  5. 2009 - Single photon emission from diamond nanocrystals in an opal photonic crystal [Crossref]
  6. 2022 - Accurate magnetic field imaging using nanodiamond quantum sensors enhanced by machine learning [Crossref]
  7. 2023 - Sensing of magnetic-field gradients with nanodiamonds on optical glass-fiber facets [Crossref]
  8. 2011 - Electric-field sensing using single diamond spins [Crossref]
  9. 2011 - Properties of nitrogen-vacancy centers in diamond: the group theoretic approach [Crossref]
  10. 2024 - Commercial nanodiamonds for precise fluorescence-based temperature sensing [Crossref]