Skip to content

Tuning electrochemical properties of 3D-printed PLA/carbon black electrodes via diamondized nanocarbon functionalization

FieldValue
JournalElectrochimica Acta
Published2026-02-01
AuthorsAna C.M. Oliveira, Raquel G. Rocha, Mariana C. Marra, Agata Rodak, Mateusz Cieślik
DOI10.1016/j.electacta.2026.148351
Citations1

The zeta potential of the diamondized nanocarbon (DNC) filler decided which 3D-printed carbon black and PLA electrode performed best. The DNC at -45 mV gave a paracetamol sensitivity of 0.406 µA·L·µmol⁻¹, about 1.45 times the 0.281 µA·L·µmol⁻¹ from the +20 mV material. Its charge-transfer resistance fell to 504.9 kΩ against 1341.6 kΩ, and the linear range widened to 300 µmol L⁻¹ from 200 µmol L⁻¹.

Three filaments shared one carbon black and PLA base and differed only in the DNC added. The particles came from Adamas Nanotechnologies and were made by controlled detonation of TNT or related explosives. Average particle size was about 200 nm and ash content about 2 wt %. Zeta potentials were -30 mV for the -COOH functionalized DNC1, +20 mV for the polyfunctional DNC2 and -45 mV for the -COOH functionalized DNC3.

Blending ran in a 2T30 screw extruder for 8 min at 100 rpm in recirculation, with barrel zones at 140, 170 and 200 °C from hopper to die. The melt left a 1.75 mm die and was air cooled into filament. A Sovol04 printed 10 × 10 mm squares, 2 mm thick, with a 0.2 mm layer, 20 mm s⁻¹ perimeter speed, a 60 °C bed and a 200 °C nozzle.

Surface treatment decided whether any signal appeared. As-printed electrodes gave no defined ferricyanide redox response, because PLA covered the conductive particles. Mechanical polishing left peak separations of 986, 1202 and 1082 mV for DNC1, DNC2 and DNC3. An air plasma pen at 3 W for 2 min, held within 1 mm of the surface, cut those values to 141, 186 and 166 mV.

Scanning electron microscopy separated the formulations before any electrochemistry ran. Negatively charged DNC1 and DNC3 composites showed a smooth untreated surface, with fillers uniformly distributed and exposed after plasma. The positive DNC2 composite already showed large clusters and voids before treatment. The authors link this to electrostatic repulsion, which keeps negative particles dispersed and lets positive ones cluster.

XPS gave the same picture in carbon fractions. Untreated surfaces were dominated by the PLA C-C/C-H component at 76.2%, 47.1% and 12.5% for DNC1, DNC2 and DNC3. Graphitic carbon was only 6.57%, 10.3% and 4.3%, and DNC3 carried 43.6% C-O. After plasma, graphitic carbon rose to 48.4%, 44.6% and 53.4%, while C-C/C-H fell to 7.3%, 9.6% and 6.7%. The plasma removed polymer and oxidized the exposed carbon.

Raman spectra showed D, G and 2D bands near 1338, 1572 and 2697 cm⁻¹ on every electrode, and the ID/IG ratio did not change. Carbon black bands mask the DNC contribution. The DNC2 electrode had a much weaker 2D band, which the authors link to poorer dispersion and greater PLA coverage of graphitic domains. Untreated contact angles sat near 67°, and plasma lowered them clearly for DNC1 and DNC3 but only slightly for DNC2.

Cyclic voltammetry used 1.0 mmol L⁻¹ [Fe(CN)₆]³⁻/⁴⁻ in 0.10 mol L⁻¹ KCl, and impedance spectra ran from 0.1 Hz to 100 kHz at +0.2 V versus Ag|AgCl|KCl(sat.). Scan rate studies from 5 to 500 mV s⁻¹ confirmed diffusion control above 20 mV s⁻¹.

ParameterDNC1, -30 mVDNC2, +20 mVDNC3, -45 mV
ΔEp (mV)141 ± 4186 ± 11166 ± 3
k0 (×10⁻⁶ cm s⁻¹)1.81 ± 0.201.32 ± 0.191.45 ± 0.38
Ae (cm²)0.15 ± 0.020.15 ± 0.010.19 ± 0.10
Rs (Ω)271.4 ± 1.5261.2 ± 1.0305.2 ± 0.6
Rct (kΩ)799.9 ± 3.31341.6 ± 3.5504.9 ± 2.9

Peak separations come from 50 mV s⁻¹ cyclic voltammograms, k0 and Ae from the scan rate study, and Rs and Rct from the Nyquist plots. The working electrode geometric area was 0.19 cm².

The -COOH functionalized materials gave the lowest charge-transfer resistance and the highest rate constants, while the polyfunctional DNC2 gave the highest resistance. The authors warn that Randles-Sevcik areas on rough composite surfaces serve as relative comparisons rather than absolute values.

DNC3 also gave the highest peak currents for dopamine and paracetamol, along with the ferricyanide pair. The mechanism proposed is electrostatic attraction between the negative surface and protonated amine groups, together with defect sites and oxygen-containing groups that lower the charge-transfer barrier.

Paracetamol detection by square-wave voltammetry

Section titled “Paracetamol detection by square-wave voltammetry”

Detection ran by square-wave voltammetry in Britton-Robinson buffer. A pH study from 2 to 12 showed current rising to pH 6 and then falling, while the oxidation peak shifted 56 mV per pH unit toward less positive potentials. That shift indicates equal numbers of protons and electrons, matching the two-proton, two-electron route to N-acetyl-p-quinone reported for paracetamol. Peak current rose linearly with the square root of scan rate and the log-log slope approached 0.5, so mass transport limited the oxidation. Final settings were amplitude 50 mV, step potential 4 mV and frequency 20 Hz. RSD stayed below 2% at both tested levels, and current and potential shifted by less than 10% between the first and the 100th cycle in 1 mmol L⁻¹ paracetamol.

The calibration comparison was the clearest result. The DNC3 electrode gave I = 0.305 + 0.406 C with R² = 0.995, sensitivity 0.406 µA·L·µmol⁻¹, a range of 1 to 300 µmol L⁻¹, LOD 0.42 µmol L⁻¹ and LOQ 1.00 µmol L⁻¹. The DNC2 electrode gave I = -0.009 + 0.281 C with R² = 0.993, sensitivity 0.281 µA·L·µmol⁻¹, a range of 1 to 200 µmol L⁻¹, LOD 0.27 µmol L⁻¹ and LOQ 0.91 µmol L⁻¹. Limits follow IUPAC rules, LOD = 3 sdB/S and LOQ = 10 sdB/S.

ElectrodeTechniqueLOD (µmol L⁻¹)Linear range (µmol L⁻¹)
Graphene/GCESWV0.0320.1 to 20
CB/PLADPV0.3701 to 200
3D-WE/BIASWASV0.2101 to 200
3D-CB/ABSDPV2.842.5 to 1158
g-C3N4/SWCNTCV0.7620 to 200
SWCNTs/PETDPV0.8191 to 2000
3D-CB/PLA/DNC3, this workSWV1.001 to 300

The comparison table lists 1.00 µmol L⁻¹ for this work, which matches the LOQ given in the text, while the text reports an LOD of 0.42 µmol L⁻¹. Lower limits elsewhere usually come from electrode preparation steps that are labour intensive, whereas the printed route needs no manual modification. Health-risk paracetamol doses of 10 g or 200 mg kg⁻¹ sit well above the linear range here.

Determination in river water, saliva and tablets

Section titled “Determination in river water, saliva and tablets”

Standard addition tested three matrices at three levels each, with three replicates. Recoveries ran 86 to 91% for river water, 91 to 103% for saliva and 95 to 102% for tablets. Most calculated Student’s t values fell below the tabulated 4.30 at 95% confidence, and three exceeded it slightly, at 5.1, 6.9 and 6.42. The authors accept these because the samples received little or no pretreatment. Five commercial tablets of 500 mg each were powdered and dissolved to 10 mmol L⁻¹, and saliva was diluted tenfold. Interferents including amoxicillin, azithromycin, dopamine, ciprofloxacin, caffeine, sodium sulphate and sodium nitrate were tested at a 1:1 ratio with no measurable shift in peak current or potential.

Zeta potential is a design variable for the filament, not only a particle descriptor. A positive DNC agglomerates inside the PLA matrix and leaves more polymer over the conductive domains, while a negative DNC disperses and lowers the charge-transfer resistance. Because charge tuning also sets the surface potential, the authors present the platform as a way to pick fillers for a target analyte.

Some limits remain. Raman cannot separate the DNC signal from carbon black, so the filler surface chemistry is only inferred, and the electroactive area values are relative. The abstract claims improved detection limits for the negative material, yet the reported LOD of 0.42 µmol L⁻¹ is higher than the 0.27 µmol L⁻¹ of the positive material. The methods section also lists a square-wave amplitude of 40 mV and a 3 mV step, while the optimization section reports 50 mV and 4 mV.

Earlier work by Cieślik and co-workers showed that DNC near 5 wt% lowered the dopamine limit below 0.18 µmol L⁻¹ against 0.48 µmol L⁻¹ for carbon black alone. The present result extends that idea from filler content to surface charge. Commercial carbon black and PLA filaments still show 2.0 to 3.5 kΩ per 10 cm, which the authors treat as the reason for custom blends.

The filler is a detonation-derived sp³ nanocarbon powder of about 200 nm, used here as a filament additive rather than a solid electrode body. For a machined diamond working electrode in the same paracetamol assay, the matching family is boron-doped diamond, supplied as plates and wafers with Au, Pt, Pd, Ti, W or Cu metallization. Single-crystal material polishes to Ra below 1 nm, and 6CCVD lists these options in the diamond materials catalog with custom geometries through the engineering support page.

View Original Abstract

This work investigates the influence of diamondized nanocarbon (DNC) surface charge on the performance of 3D-printed CB/PLA electrodes for paracetamol detection. Three filaments were prepared by the thermal method, incorporating DNCs with different zeta potentials, one positive (+20 mV) and two negative (-30 mV and -45 mV). Surface characterization by XPS and Raman spectroscopy revealed that DNC charge affects dispersion, polymer coverage, and the exposure of carbon black domains, whereas SEM images showed that positively charged DNCs tend to aggregate, whereas negatively charged DNCs remain well-dispersed. Contact angle measurements indicated increased hydrophilicity for electrodes containing negatively charged DNCs. Electrochemical analysis demonstrated lower charge-transfer resistance and superior current response for these electrodes, with an extended linear range and improved detection limits for paracetamol (∼1.5 times higher than positively charged DNCs). Overall, the results highlight that the DNC zeta potential is a key parameter for optimizing 3D-printed electrodes, providing a simple, low-cost strategy for the fabrication of portable and high-performance electrochemical sensors. Importantly, this is the first report demonstrating that DNC zeta potential significantly influences filament synthesis for electrochemical applications, opening new opportunities for the incorporation of various nanoparticles into filament composite.

  1. 2025 - Electrochemical methods for the determination of acetaminophen in biological matrices: a critical review in the clinical field [Crossref]
  2. 2022 - Emerging contaminants of high concern for the environment: current trends and future research [Crossref]
  3. 2016 - Lessons learned from more than two decades of research on emerging contaminants in the environment [Crossref]
  4. 2018 - Paracetamol - toxicity and microbial utilization. Pseudomonas moorei KB4 as a case study for exploring degradation pathway [Crossref]
  5. 2016 - Possible ecological risk of two pharmaceuticals diclofenac and paracetamol demonstrated on a model plant Lemna minor [Crossref]
  6. 2023 - Paracetamol detection in environmental and pharmaceutical samples using multi-walled carbon nanotubes decorated with silver nanoparticles [Crossref]
  7. 2025 - Development of an electrochemical sensor for the detection of paracetamol using graphitic carbon nitride and single-walled carbon nanotubes [Crossref]
  8. 2022 - Editors’ Choice—Review—3D printing: an innovative trend in analytical sensing [Crossref]
  9. 2020 - A scientist’s guide to buying a 3D printer: how to choose the right printer for your laboratory [Crossref]
  10. 2022 - The effect of water ingress on additively manufactured electrodes [Crossref]