Uncovering origins of heterogeneous superconductivity in La3Ni2O7
Paper details
Section titled “Paper details”| Field | Value |
|---|---|
| Journal | Nature |
| Published | 2026-02-25 |
| Authors | S. V. Mandyam, E. Wang, Z. Wang, B. Chen, N. C. Jayarama |
| DOI | 10.1038/s41586-025-10095-x |
| Citations | 5 |
Local shear stress above approximately 2 GPa quenched superconductivity in La3Ni2O7, according to wide-field nitrogen-vacancy magnetometry performed inside a diamond anvil cell. The study mapped the Meissner response, normal stress, shear stress, and La:Ni composition at sub-μm resolution. At a mean normal stress of 21 GPa, sample S1 reached a diamagnetic transition temperature of about 80 K. Its first superconducting patch appeared near a local normal stress of 17.5 GPa.
Local controls on superconducting behavior
Section titled “Local controls on superconducting behavior”The paper reports pressure as averaged normal stress, σZZ, because each sample experienced a distribution of local stresses. The phase diagram therefore uses a continuous local axis instead of treating each cell load as one uniform state.
| Result | Condition | Reported value | Basis |
|---|---|---|---|
| Diamagnetic onset | S1, mean σZZ of 21 GPa | Tc ≈ 80 K | ODMR and resistance |
| Diamagnetic onset | S1, mean σZZ of 25 GPa | Tc ≈ 65 K | ODMR and resistance |
| First superconducting patch | S1, mean σZZ of 16 GPa | Local σZZ ≈ 17.5 GPa | ODMR stress map |
| Critical shear | Pooled S1-S3 data, T ≤ 35 K | Approximately 2 GPa | ODMR stress correlation |
| Local diamagnetism | S3, mean σZZ of 21 GPa | Tc ≈ 60 K without a global resistance drop | ODMR |
| Superconducting volume fraction | S1, S2, and S3 | 3%, 0.3%, and 0.5% | Stray-field model |
Pixel registration across S1-S3 produced a stress-temperature dome in excellent agreement with earlier phase diagrams. The pooled normal-stress analysis used pixels of the order of one million. The chemical map of S1 did not by itself explain its annular magnetic response. Shear supplied the missing correlation.
Wide-field measurement inside a diamond anvil cell
Section titled “Wide-field measurement inside a diamond anvil cell”Three independent floating-zone-synthesized La3Ni2O7 single crystals, labelled S1, S2, and S3, were mounted in separate diamond anvil cells. Each crystal sat in NaCl pressure medium within an insulating cBN gasket and connected to platinum transport leads.
The top anvil was synthetic type Ib [111]-cut diamond. A shallow layer of nitrogen-vacancy centres lay about 500 nm below the culet surface at a density of approximately 1 ppm.
The layer was produced with carbon-12 ion implantation at energies up to 450 keV and doses up to 9.9 × 10¹¹ cm⁻². Vacuum annealing above 850 °C for 12 h below 10⁻⁶ mbar allowed vacancies to form nitrogen-vacancy centres probabilistically.
A 532 nm excitation laser and microwave readout produced wide-field ODMR maps of local magnetic fields and stresses with sub-μm resolution. Four-probe resistance was recorded during selected magnetometry sequences.
Diamagnetism agrees with transport
Section titled “Diamagnetism agrees with transport”The diamagnetism sequence began with zero-field cooling, followed by applying a field along Z and warming in steps. Applied fields were typically 100 to 150 G.
Nitrogen-vacancy centres above the sample measured the magnetic ratio s = B/H. Values below 1 mark field suppression above diamagnetic regions. Values above 1 mark field enhancement at edges, while distant regions returned s ≈ 1.
At mean σZZ of 21 GPa, one interior point held s ≈ 0.95 from 20 K to 50 K. An edge point held s ≈ 1.05 over the same interval. The points converged near s = 1 at about 80 K.
At 25 GPa, they converged near 65 K. Both temperatures matched the first drop in resistance.
S2 produced similar but weaker and smaller diamagnetic regions. Its transport transition began at mean σZZ of 13 GPa.
For flux trapping, the authors field-cooled S1 to 20 K under 150 G and quenched the field to zero. Remnant fields reached around 10 G and coincided with the strongest diamagnetism. The authors report this as the first observation of flux trapping in nickelates. They interpret the overlap as evidence that superconducting regions supplied paths for trapped flux.
Normal and shear stress separate onset from suppression
Section titled “Normal and shear stress separate onset from suppression”At mean σZZ of 16 GPa, S1’s local normal stress ranged from 13 GPa to 18 GPa. First signatures of superconductivity occupied an area with local stress above 17 GPa. Figure 4 places that region near 17.5 GPa.
At 21 GPa, the central hole in the diamagnetic response did not follow the normal-stress map. It instead aligned with high shear.
The authors decomposed boundary traction into normal stress σZZ and shear stress τ. The shear magnitude combines the σXZ and σYZ components. Traction is continuous across the diamond-sample interface, so the NV map describes stress transmitted into La3Ni2O7.
Above a critical shear of approximately 2 GPa, superconducting behaviour quenched. Pooled pixel data produced a superconducting dome in the normal-stress and shear-stress plane. They also constructed a three-dimensional phase diagram in temperature, normal stress, and shear stress.
Ruby pressure was about 0.73 of averaged normal stress and missed several-GPa local variations. Stress gradients did not correlate with absent superconductivity.
Stoichiometry filters local superconductivity
Section titled “Stoichiometry filters local superconductivity”S3 was chosen for strong spatial La:Ni inhomogeneity. It contained two Ni-enhanced stripes far from the 3:2 ratio.
At mean σZZ of 21 GPa, global resistance showed no visible drop. Yet at 9 K, ODMR found weak local pockets of diamagnetic suppression. The pockets vanished above Tc ≈ 60 K.
EDX registration showed no diamagnetic response where La:Ni departed from 3:2. Nearly all regions at 3:2 showed weak diamagnetism. EDX used 15 keV electrons at 60 mA, with La2O3 and Ni standards for calibration.
For S1, EDX found regular Ni-rich inclusions at a few-micrometre scale and smaller La-rich regions. That chemical texture alone did not explain S1’s bulk magnetic features.
Different Ruddlesden-Popper phases with distinct La:Ni ratios compete during crystal growth. The data support stoichiometry as one local control alongside stress.
Limits and unresolved mechanisms
Section titled “Limits and unresolved mechanisms”The reported volume fractions are model estimates, not direct measurements. The calculation assumes superconducting material has χSC = -1 and the remainder has χPM ≈ 0.
Earlier studies using conventional susceptibility measurements reported volume fractions above 40% for the most hydrostatic media, including helium. The lower estimates agree with shear suppressing superconductivity, but they do not establish its microscopic cause.
The mechanism by which shear destroys superconductivity remains open. The authors list plastic deformation and shear distortion of the Ni-O bond angle as possibilities. That angle controls coupling between bilayers, but neither mechanism was tested directly.
Variability in S2 also remains unexplained. Oxygen stoichiometry and layer stacking variations are candidate causes for future imaging. Paramagnetic regions may represent the Wohlleben effect, but that interpretation remains tentative.
Shear extraction used four D values rather than a full tensor reconstruction. Comparison against the 4D+2E method gave τ(4D) = (1.8 ± 0.2) × τ(4D+2E). The three-dimensional boundary also used spline extrapolation to zero on all axes.
Implications for high-pressure engineering
Section titled “Implications for high-pressure engineering”A single bulk pressure cannot predict where La3Ni2O7 will superconduct. Sample and cell design should therefore monitor local normal stress, shear stress, and La:Ni ratio.
Global four-probe resistance can miss local superconducting pockets, as S3 demonstrated. Local magnetic mapping can distinguish weak active regions from inactive volume.
For high-pressure metrology, the authors treat sample inhomogeneity as a set of many micrometre-scale samples. This approach converts stress gradients and compositional variations into measured phase-diagram coordinates.
Pressure-cell qualification should therefore include local stress and stoichiometry maps. It should not rely only on ruby pressure and nominal La3Ni2O7 composition.
Materials and support
Section titled “Materials and support”The high-pressure sensor requires a type Ib [111]-cut single-crystal diamond anvil with a shallow nitrogen-vacancy layer and platinum elements for microwave excitation and transport contacts.
6CCVD’s diamond materials catalog includes single-crystal diamond grown by MPCVD and Pt metallization, corresponding to the substrate and conductor families in the reported sensor.
The linked engineering support page can be used to discuss the paper’s anvil geometry, nitrogen-vacancy layer, and metal integration.
View Original Abstract
Abstract The family of nickelate superconductors have long been explored as analogues of the high-temperature cuprates 1-6 . Nonetheless, the recent discovery that certain stoichiometric nickelates superconduct up to high critical temperatures ( T c ) under pressure came as a surprise 7-13 . The mechanisms underlying the superconducting state remain experimentally unclear. Apart from the practical challenges posed by working in a high-pressure environment, typical samples exhibit anomalously weak diamagnetic responses, which have been conjectured to reflect inhomogeneous ‘filamentary’ superconducting states 7,9,14-17 . Here we perform wide-field, high-pressure, optically detected magnetic resonance spectroscopy to image the local diamagnetic responses of as-grown La 3 Ni 2 O 7 samples in situ, using nitrogen vacancy quantum sensors embedded in the diamond anvil cell 18-23 . These maps confirm marked inhomogeneity of the functional superconducting responses at the few μm scale. By spatially correlating the diamagnetic Meissner response with both the local tensorial stress environment, also imaged in situ, and stoichiometric composition, we show the dominant mechanisms suppressing and enhancing superconductivity. Our wide-field technique simultaneously provides a broad view of sample behaviour and excellent local sensitivity, enabling the rapid construction of multi-parameter phase diagrams from the local structure-function correlations observed at the sub-μm pixel scale.
Electronic Grade Intrinsic Diamond Epitaxial Wafer H Terminated Superior 100 Mosfet Ready Substrate
View Specs →Products
View Specs →
Single Crystal Cvd Diamond Plate
View Specs →References we cover
Section titled “References we cover”- The Paramagnetic Meissner Effect (PME) in Metallic Superconductors
- Scanning nitrogen-vacancy magnetometry down to 350 mK
- Widefield quantum microscopy with nitrogen-vacancy centers in diamond -n strengths, limitations, and prospects
- Magnetometer with nitrogen-vacancy center in a bulk diamond for detecting magnetic nanoparticles in biomedical applications
- Nanomechanical Sensing Using Spins in Diamond
Citing papers we cover
Section titled “Citing papers we cover”- Construction optimization and functional applications of fluorescent nanodiamonds
- Probing the Meissner effect in single crystals of Bi2Sr2Ca2Cu3O10+δ via wide-field quantum microscopy under high pressure