Heterostructured B-C particles - Bridging solid and mesoporous domains
Paper details
Section titled “Paper details”| Field | Value |
|---|---|
| Journal | Journal of Applied Physics |
| Published | 2026-03-11 |
| Authors | A. Yu. Basharin, V. S. Dozhdikov, G. V. Belov, A. L. Vasiliev |
| DOI | 10.1063/5.0304129 |
Single-pulse laser processing produced 0.5 to 15 μm B-C microparticles with two structural domains. A 14 μm particle contained a 0.9 μm mesoporous belt with 4.7 ± 0.5 at.% boron. Its dense core contained about 21 at.% boron. The belt formed from supersaturated boron-doped carbon, while the core contained a hypereutectic C-B4.5C mixture. The authors attributed the two-domain structure to local supercooling, which suppressed boron diffusion near the diamond interface.
Particle architecture
Section titled “Particle architecture”SEM showed nearly spherical particles in the laser exposure zone. The analyzed particle measured 14 μm in diameter. FIB sectioning produced a 14 × 5 × 5 μm³ lamella that included the particle and underlying diamond. The 300 kV TEM and STEM used EDXS, EELS, SAED, and HRTEM. The 0.9 μm mesoporous layer was the rapidly quenched (RQ) interface. The upper body was the quasi-equilibrium-solidified (QES) core. The authors treated the solid particle as one object containing both RQ and QES regions.
Laser process and substrate conditions
Section titled “Laser process and substrate conditions”The starting mixture contained HOPG flakes and amorphous boron at a B/C weight ratio of 13:87. The boron purity exceeded 99.2 wt.%, and oxygen was below 0.5 wt.%. Mg, Fe, and Si totaled less than 0.3 wt.%. Ball milling for 10 min produced HOPG flakes with lateral sizes of 1 to 150 μm. The mixture was pressed onto a 1 × 3 mm² polycrystalline CVD diamond film. Some mixture remained on protruding diamond grains with predominant (100) and (110) orientations. The chamber contained helium at 25 MPa. A solid-state Nd-doped glass laser delivered one 1.06 μm pulse with 5 J energy, a 1 mm spot, and 1 ms duration. The particle side faced the entrance window, and the beam passed through it. SEM used a 1 kV accelerating voltage in low vacuum to reduce charging. EDXS identified carbon-rich particles and one boron-enriched particle with C:B ≈ 2.4:1. Large particle sizes ranged from 0.5 to 15 μm.
Interface composition and crystal phases
Section titled “Interface composition and crystal phases”The rapidly quenched interface contained four zones from the diamond upward. An amorphous carbon layer touched the diamond. A nonporous region of randomly oriented nanographite crystallites lay above it. The crystallites were about 1 nm, and the next zone held fused onion-like carbon particles. The onion-like particles were 4 to 7 nm across, with layer spacings of 0.34 to 0.37 nm. Graphite ribbons formed the upper zone and contained rare rhombohedral boron carbide inclusions. EELS measured the onion-like region as B4.7C95.3, corresponding to 4.7 ± 0.5 at.% boron. Electron diffraction confirmed disordered graphite in the mesoporous belt. HRTEM found no free boron in the interface, which supports substitutional boron within the carbon network. Electron diffraction also showed that the underlying CVD diamond did not graphitize. The dense core had a mosaic structure rather than uniform boron carbide. A 600 nm faceted crystal matched rhombohedral B4C by selected-area electron diffraction. Stacking faults ran parallel to the B4C basal planes. Fast Fourier transform patterns showed disordered B4C at the core edge. The refined carbide composition was B4.5C, while the average core composition was about 21 at.% boron. The core was a hypereutectic mixture of B4.5C and boron-free graphite. The carbide was dense and nonporous, while adjacent graphite contained lenticular and shrinkage pores.
Condensation, supercooling, and wetting
Section titled “Condensation, supercooling, and wetting”Vapor condensation on diamond followed a vapor-liquid-crystal route, rather than homogeneous nucleation in helium. Spherical particle shapes and the absence of dendritic or fractal forms supported that interpretation. Deep supercooling was associated with high viscosity and reduced time for boron redistribution. The authors proposed that separate rapidly quenched nanodroplets left pores between them after solidification. This sequence produced the mesoporous belt and prevented boron carbide formation there. The cited upper value for CVD diamond thermal conductivity was 2 kW/mK. The cross-plane conductivity of HOPG was 3.3 W/mK. The authors attributed the difference in condensation behavior to this thermal contrast. At a bifurcation point, latent heat overheated particles on graphite and stopped individual droplet growth. Condensation then produced monodisperse arrays with a diameter of about 150 nm. The hydrophobic mesoporous layer supported a Cassie-Baxter state, which helped preserve the spherical shape. Observed particles also included intermediate wetting and a Cassie-to-Wenzel transition.
Molecular dynamics of the boron-doped belt
Section titled “Molecular dynamics of the boron-doped belt”Molecular dynamics addressed the atomic structure of the 4.7 at.% boron solid solution. LAMMPS used a machine-learning Gaussian approximation potential verified from 300 to 5000 K. The cubic cell contained 12,548 atoms, with 4.7% assigned to boron. Under NPT conditions at 25 MPa, the cell cooled from 6000 to 300 K at 10^14 K/s. The final bond-angle peak near 120° matched sp2 carbon in graphene-like planes. Six-membered rings outnumbered five- and seven-membered rings. The model contained no free carbon or boron atoms. Boron distorted the ring planes and produced five- and seven-membered ring motifs. The authors associated pentagons with positive curvature and heptagons with negative curvature. They connected these structures to onion-like carbon formation and pores near the particle-diamond interface.
Comparison with equilibrium and unresolved questions
Section titled “Comparison with equilibrium and unresolved questions”The measured 4.7 at.% boron exceeds the cited equilibrium solubility of 2.3% at 2650 K. The mesoporous belt was therefore a supersaturated substitutional solid solution. The cited prior study reported onion-like carbon at boron concentrations up to 5 or 6 at.%. The measured 4.7 at.% concentration falls below that cited range. At 25 at.% boron, that cited work reports a graphite-like C75B25 compound. The authors linked the dense core to quasi-equilibrium solidification and phase separation consistent with the B-C diagram. They describe the 0.5 to 15 μm particles as unusually large for laser condensation in buffer gas. Quantitative Cassie-Baxter analysis was not possible because the water contact angle on HOPG depends on surface condition. Reported water contact angles range from 37° for annealed HOPG to 119° for contaminated HOPG. The particle contact angle reached 158°, while the porous interface changed the wetting state. Particle adhesion to diamond was weak, with visible delamination and easy removal by a squirrel hair brush. The nanoscale zoning was resolved mainly in one 14 μm particle, so variation across many particles was not quantified. Stabilization, encapsulation, loading and release, and biocompatibility remain untested for biomedical use. The authors present boron neutron capture and targeted drug delivery as proposed uses, not demonstrated functions.
Implications for diamond processing
Section titled “Implications for diamond processing”Diamond served as a process component because its thermal conductivity and grain relief controlled condensation and quenching. Reproducing the method requires a rough, thermally conductive CVD diamond surface and control of chamber pressure and pulse energy. The reported window used helium at 25 MPa, one 1 ms pulse, and a B/C ratio of 13:87. Weak particle adhesion must be considered during collection and handling. For composite integration, the dense B4.5C-C core and porous carbon belt should be treated as distinct material domains. The study did not measure particle transport, surface area, loading and release, or biocompatibility. Any device claim based on those properties requires separate testing.
Materials and support
Section titled “Materials and support”For laser condensation at 25 MPa, the process needs a coarse-grained polycrystalline CVD diamond substrate; the study used a 1 × 3 mm² film. 6CCVD’s diamond materials catalog lists MPCVD-grown single-crystal and polycrystalline diamond plates and wafers up to 125 mm. Use engineering support to define the specimen geometry and grain surface required for the process.
View Original Abstract
Microparticles comprising two macroscopically distinct domains with different compositions, structures, and porosity are attractive as multifunctional materials. B-C microparticles with dual-domain structures were synthesized via single-pulse laser heating of graphite-boron mixtures on chemical vapor deposition diamond. Vapor condensation forms Cassie-Baxter droplets featuring two distinct regions: a near-contact, mesoporous rapidly quenched (RQ) boron-doped onion-like carbon (OLC) network (∼4.7 at. % B) and a dense, quasi-equilibrium (QE) hypereutectic C-B4.5C mixture. Molecular dynamics simulations support the RQ structure. The results demonstrate that local supercooling suppresses boron diffusion, enabling the coexistence of mesoporous and dense domains within a single heterostructured microparticle.
Free Standing Boron Doped Diamond Pcd Film
View Specs →
Boron Doped Single Crystal Diamond Plate
View Specs →
Single Crystal Cvd Diamond Plate
View Specs →Original source
Section titled “Original source”References
Section titled “References”- 2012 - Solidification and Crystallization Processing in Metals and Alloys
- 2005 - Measurements of the melting point of graphite and the properties of liquid carbon (a review for 1963-2003) [Crossref]
- 2004 - Methods of increasing the measurement accuracy during the experimental determination of the melting point of graphite [Crossref]
- 1976 - Graphite-liquid-vapor triple point pressure and the density of liquid carbon [Crossref]
- 2025 - Graphite melting and the nature of liquid carbon [Crossref]
- 2007 - Metastable Solids from Undercooled Melts
- 2009 - Phases formed during rapid quenching of liquid carbon [Crossref]
- 2022 - Quenching of liquid carbon on the surface of a diamond substrate [Crossref]
- 2010 - Synthesis and consolidation of boron carbide: A review [Crossref]
- 2000 - Evidence for the solubility of boron in graphite by electron energy loss spectroscopy [Crossref]