Magnetic sensing and imaging using nanodiamond NV center films and microwave integration into an STM coplanar waveguide stage
Paper details
Section titled “Paper details”| Field | Value |
|---|---|
| Journal | Japanese Journal of Applied Physics |
| Published | 2026-03-16 |
| Authors | Toyo Kazu Yamada, Achmad Yahiya Koki, Mai Niida |
| DOI | 10.35848/1347-4065/ae4a30 |
Drop-cast nanodiamond films imaged a credit card’s stray fields at micrometer scale under ambient conditions. A redesigned STM coplanar waveguide delivered more than 90% of incident microwave power across 2 to 3 GHz. The reported work confirms ODMR operation on an STM-compatible stage, but simultaneous SP-STM and ODMR measurements remain under development.
Nanodiamond sensing layer
Section titled “Nanodiamond sensing layer”Spin-polarized STM can resolve individual magnetic atoms, but it does not directly sense magnetic fields. NV centers provide complementary stray-field sensitivity through optically detected magnetic resonance. The negatively charged NV− center has an S = 1 ground state split by a zero-field splitting of about 2.87 GHz. Under 532 nm excitation, radiative relaxation produces red photoluminescence centered at 637 nm. Resonance increases nonradiative decay through an intermediate singlet, which reduces the observed intensity.
The authors formed the sensing layer by drop-casting carboxylated nanodiamond solution onto glass. They deposited 5 μL at 1 mg mL−1 over an area of 2 × 2 mm2 and dried the film in air. The average particle diameter was approximately 100 nm. At an NV concentration of about 3 ppm, each particle contained approximately 300 NV centers.
Randomly oriented NV spin axes made the film responsive to fields with arbitrary directions. That geometry also limits the image to variations in local field amplitude rather than vector components. Typical nanodiamonds have diameters of 50 to 200 nm. Particles below 10 nm tend to host less stable NV centers, which reduces their sensitivity. Finite particle size limits the reported spatial resolution to micrometer scales. SP-STM retains atomic-scale spin imaging, while the nanodiamond film supplies complementary long-range field information.
ODMR setup and microwave readout
Section titled “ODMR setup and microwave readout”A conventional optical microscope supplied excitation, collection, and microwave access to the film. Light from a 532 nm continuous-wave laser passed through a half mirror and a 0.4 numerical aperture objective. Photoluminescence above 650 nm reached a Basler CMOS camera after a long-pass filter. A Python program controlled a voltage-controlled oscillator over 2.7 to 3.1 GHz. Amplified microwave power reached a home-built copper-coated PCB coplanar waveguide, with the film placed directly on it.
The key acquisition conditions were as follows.
| Component | Paper condition |
|---|---|
| Excitation | 532 nm continuous-wave laser; objective numerical aperture 0.4 |
| Microwave | 10 dBm, equivalent to 10 mW; oscillator range 2.7 to 3.1 GHz |
| Detection | Long-pass filter above 650 nm; Basler 720 × 540 pixel CMOS camera |
| Normalization | Microwave-on photoluminescence divided by microwave-off photoluminescence at each frequency |
| Sample | Direct contact between the drop-cast film and copper-coated PCB CPW |
Continuous-wave operation and slight optical defocusing required a relatively high initial laser power. This requirement follows from the nonequilibrium spin polarization used to generate ODMR contrast. Normalizing microwave-on and microwave-off photoluminescence compensated for laser intensity fluctuations.
Microwave field above the coplanar waveguide
Section titled “Microwave field above the coplanar waveguide”Lateral film shifts showed that the microwave field extended more than 3 mm from the CPW center. Two ODMR dips appeared near y = ±1 mm, close to the conductor edges. These locations indicate preferential microwave spreading from the strip edges.
Vertical scans showed gradual signal decay as the film moved away from the CPW surface. The authors report a field extent of approximately 8 mm from that surface. They therefore identify a magnet thickness of 0 to 2 mm as suitable for effective microwave application. Standoff and lateral position must therefore be controlled during imaging.
Magnetic response and domain imaging
Section titled “Magnetic response and domain imaging”Home-built Helmholtz coils applied an in-plane x-axis field from 0 to 2 mT. An electromagnet applied an out-of-plane z-axis field from 0 to 7 mT. The film and CPW stayed at y = 0 mm and z = 0 mm during both scans. The ODMR dips changed continuously with field strength in both orientations.
For the in-plane field, both dips varied with an application of approximately 0.1 mT within a 50 ms averaging time. At 2.8704 GHz, intensity changed little from 0.0 to 0.4 mT, then increased linearly above 0.5 mT. At 2.8640 GHz, intensity decreased up to 0.7 mT and then increased linearly at higher fields.
For the out-of-plane field, intensities near 2.8704 and 2.8640 GHz decreased below 1 mT and increased above 1 mT. The fitted dependence was quadratic for the out-of-plane response. The dip tails also shifted with field, and quadratic fits described those variations. Contrast differed between the two scans because the authors changed defocusing and nanodiamond positioning. This difference cannot be assigned to field orientation alone.
Imaging used a 20× objective and produced a 590 μm × 440 μm CMOS image area. One raw frame contained 720 × 540 pixels and used a 50 ms exposure. Signal was averaged into 36 × 27 blocks, each covering 20 × 20 pixels. The microwave frequency was set to 2.8640 GHz, where field-induced intensity changes were pronounced.
The sample was a credit card with an approximately 0.09 mT out-of-plane surface stray field, measured by a Hall probe. Stripe-like domains appeared in the x-by-y map and rotated with the card after a 90° rotation. This response confirms that the domains came from the card’s stray field. The random NV axes still prevent direct reconstruction of the local vector field.
STM coplanar waveguide stage
Section titled “STM coplanar waveguide stage”The initial PCB CPW measured 70 × 19 mm, with a 1.6 mm substrate and 0.018 mm copper on both faces. It was too large for a 15 × 15 mm STM stage, and repeated mounting prevented direct SMA contact. All configurations were tested from 2 to 3 GHz with a vector network analyzer.
The configurations produced the following transmission and reflection results.
| Configuration | Connection | Result from 2 to 3 GHz |
|---|---|---|
| Standard PCB CPW | Two SMA terminals | About 10% to 40% transmitted |
| Prototype 1 | Metal tube and nickel ribbon | 20% to 80% reflected |
| Prototype 2 | Stainless-steel coaxial cable, 50 pF m−1 | 20% to 60% reflected |
| Prototype 3 | One SMA and 50 Ω ground termination | More than 90% transmitted |
Prototype 3 removed the second terminal and used one SMA connector with a 50 Ω load connected to ground. This configuration established stable contact through a nickel ribbon and a 2 mm neodymium magnet. The magnet was positioned more than 5 mm from the diamond. Annealing it in air at 523 K for 5 min reduced the field from 2.4 mT to 0.7 mT at 5 mm. A bulk single-crystal CVD diamond sample then produced a well-defined ODMR spectrum on the stage.
Path to combined SP-STM and ODMR
Section titled “Path to combined SP-STM and ODMR”The authors describe the combined instrument as a setup under development. Its CPW uses a copper film on PCB with a central aperture, or a transparent glass or sapphire substrate. Drop-cast nanodiamonds form the sensing layer on that substrate.
A conductive two-dimensional overlayer, such as a two-dimensional magnet or graphene, carries tunneling current. The overlayer must preserve an atomically flat surface for SP-STM. ODMR would then sense stray fields while SP-STM reads local spin polarization. The paper does not report a simultaneous dataset from this assembly. It therefore demonstrates the sensing and microwave-delivery components separately, not the completed correlative measurement.
Limits and engineering implications
Section titled “Limits and engineering implications”The random NV orientations make the film suitable for field directions that need not be known in advance. They also restrict each camera value to a scalar contrast rather than a vectorial field component. Finite particle size limits spatial resolution to micrometer scales, whereas SP-STM retains atomic-scale spin contrast. Magnetic force microscopy offers typical 10 to 50 nm spatial resolution, as cited in the paper. The ND platform therefore complements, rather than replaces, higher-resolution magnetic probes.
Low-field response is nonmonotonic around zero, while higher-field intensity changes were linear or quadratic depending on orientation. The paper does not report an absolute sensitivity calibration or a vector-field reconstruction. Optical defocusing, film placement, and laser power also changed the contrast.
The STM design further requires control of magnetic contamination from the neodymium coupling magnet. The measured CPW field geometry limits where samples can sit without losing microwave coupling. For engineering selection, use drop-cast nanodiamond films for ambient magnetic-domain imaging and reserve SP-STM for atomic-scale spin information. For the STM stage, validate microwave transmission, sample standoff, and magnetic background before interpreting ODMR contrast.
Materials and support
Section titled “Materials and support”For STM-stage validation, ODMR requires a bulk single-crystal CVD diamond sample containing NV centers. The 6CCVD diamond materials catalog lists MPCVD-grown single-crystal plates and wafers up to 125 mm. The engineering support link provides custom fabrication support for assessing CPW sample geometry, subject to confirming NV concentration and film specification.
View Original Abstract
Abstract Spin-polarized scanning tunneling microscopy (SP-STM) enables access to the spin polarization of individual magnetic atoms but is inherently insensitive to magnetic fields. In contrast, nitrogen-vacancy (NV) centers in diamond provide highly sensitive magnetic-field detection through optically detected magnetic resonance (ODMR). Integrating ODMR-based magnetic-field sensing with SP-STM therefore offers a pathway to comprehensive magnetic characterization from the atomic scale to long-range fields. Here, we demonstrate that drop-cast nanodiamond (ND) films with an average particle size of ~100 nm deposited on glass substrates function as magnetic-field sensors for imaging magnetic domains under ambient conditions using a conventional ODMR setup. The random orientations of NV centers in the ND ensemble enable detection of magnetic fields with arbitrary directions without crystallographic alignment. Furthermore, we report progress toward integrating ODMR with SP-STM by developing an STM stage equipped with a coplanar waveguide, enabling reliable microwave delivery to the STM junction.
Single Crystal Cvd Diamond Plate
View Specs →
Diamond Heat Spreader With Copper Coated Metalized Surface
View Specs →
Customized Single Crystal Cvd Diamond Plate
View Specs →References we cover
Section titled “References we cover”- Nanodiamonds enable femtosecond-processed ultrathin glass as a hybrid quantum sensor
- Wide-field fluorescent nanodiamond spin measurements toward real-time large-area intracellular thermometry
- Real-time estimation of the optically detected magnetic resonance shift in diamond quantum thermometry toward biological applications
- Sensitivity optimization for NV-diamond magnetometry
Original source
Section titled “Original source”References
Section titled “References”- 2004 - Step-induced frustration of antiferromagnetic order in Mn on Fe(001) [Crossref]
- 2003 - Observation of spin-polarized surface states on ultrathin Bct Mn(001) films by spin-polarized scanning tunneling spectroscopy [Crossref]
- 2003 - Origin of magnetic contrast in spin-polarized scanning tunneling spectroscopy: experiments on ultra-thin Mn films [Crossref]
- 2002 - Magnetic force microscopy study of electron-beam-patterned soft permalloy particles: technique and magnetization behavior [Crossref]
- 2002 - MFM study of magnetic Vortex cores in circular permalloy dots: behavior in external field [Crossref]
- 2022 - High-resolution alternating magnetic force microscopy using an amorphous FeB-Based tip driven by an inverse magnetostrictive effect: imaging of the high-density magnetic recording media [Crossref]
- 1999 - Exchange coupling in magnetic multilayers grown on iron whiskers [Crossref]
- 1999 - !Ect of roughness, frustration, and antiferromagnetic order on magnetic coupling of Fe/Cr multilayers [Crossref]
- 1993 - Optical detection of magnetic resonance in a single molecule [Crossref]
- 2020 - Sensitivity optimization for NV-diamond magnetometry [Crossref]