A review of cutting tool materials in metal cutting processes
Paper details
Section titled “Paper details”| Field | Value |
|---|---|
| Journal | Discover Applied Sciences |
| Published | 2026-05-23 |
| Authors | Abhijit Saha, Rajeev Ranjan, Alemu Workie Kebede, Himadri Majumder |
| DOI | 10.1007/s42452-026-08879-5 |
The review places PCD at the top of the compared tool materials for room-temperature hardness, with a value above 70 GPa. It also reports about 50 to 70 GPa at 700 °C and thermal conductivity of 400 to 700 W/m·K. These properties support PCD use in non-ferrous and abrasive-material machining. They do not make PCD a universal choice. The review ties selection to workpiece chemistry, cutting temperature, load continuity, geometry, and cost.
Review method and evidence
Section titled “Review method and evidence”The review drew from publications dated 1990 through 2025 and included 104 eligible peer-reviewed papers. Searches covered Scopus, Web of Science, Elsevier, Springer Nature, Taylor & Francis, and Google Scholar. The eligibility criteria required peer-reviewed journal articles in English. The authors did not produce a new machining dataset. Their evidence came from separate studies reporting tool life, wear, cutting force, surface finish, dimensional accuracy, and residual stress. Sources covered turning, milling, drilling, grinding, and coating tests. Property figures and tables combine results from different studies and operating conditions.
Hardness, toughness and thermal behavior
Section titled “Hardness, toughness and thermal behavior”PCD’s room-temperature hardness exceeded 70 GPa, but its fracture toughness was lower than that of WC-Co carbides. WC-Co combined hardness of 15 to 22 GPa with fracture toughness of 8 to 15 MPa·m^1/2. The review’s quantitative table gives these reported values:
| Tool material | Reported hot hardness | Thermal conductivity (W/m·K) | Thermal expansion (×10⁻⁶/K) |
|---|---|---|---|
| High-speed steel | About 4 to 6 GPa at 600 °C | 20 to 30 | 10 to 13 |
| Cemented carbide | About 10 to 15 GPa at 800 °C | 80 to 110 | 4.5 to 6.5 |
| Al₂O₃-based ceramic | About 15 to 20 GPa at 1000 °C | 20 to 35 | 7 to 8 |
| Cubic boron nitride | About 30 to 40 GPa at 1000 °C | 60 to 130 | 4 to 5 |
| Polycrystalline diamond | About 50 to 70 GPa at 700 °C | 400 to 700 | 1 to 2 |
PCD therefore has the highest thermal conductivity and lowest thermal expansion in the table. CBN reaches 30 to 40 GPa at 1000 °C, a higher temperature than the 700 °C PCD comparison. WC-Co’s toughness makes it suitable for interrupted cutting, while PCD and CBN need more careful load control. Hot hardness alone does not establish the best tool for a given cut.
Wear mechanisms govern service conditions
Section titled “Wear mechanisms govern service conditions”At the tool-chip interface, contact pressures reach 1 to 3 GPa. Temperatures can exceed 800 to 1000 °C, depending on cutting speed and workpiece. Abrasive wear occurs when hard workpiece phases cut or plough the tool. Adhesive wear comes from repeated junction formation and rupture at the interface. Diffusion wear transfers atoms across the interface under thermal activation. Oxidative wear results from tribochemical reactions with atmospheric oxygen. The modes often act together, so a coating that controls one mechanism may not control the others.
PCD is chemically reactive with ferrous materials at elevated temperatures because carbon can dissolve into iron. This accelerates crater wear and makes PCD unsuitable for ferrous machining. CBN has lower iron affinity, although chemical and diffusion degradation can still occur during high-speed or dry cutting. One cited study reported 4 to 5 times longer CBN tool life than diamond for iron-based alloys and hardened steels. The review did not reproduce that comparison in a shared experiment.
Coatings affect hot hardness and oxidation resistance
Section titled “Coatings affect hot hardness and oxidation resistance”PVD and CVD put a hard layer on a tougher substrate. PVD operates below the HSS tempering temperature, so the tool does not need heat treatment after coating. CVD can deposit dense, high-purity layers and multiple Al₂O₃ or TiN layers over Al₂O₃ or TiC. TiAlN can form protective Al₂O₃ scales, while AlCrN can form Cr₂O₃. These scales slow oxidation at high temperatures. Common nanocomposite nc-TiN/a-Si₃N₄ coatings use grains below 10 nm in an amorphous matrix. The matrix restricts grain growth and dislocation motion. Reported nanocomposite hardness exceeds 40 GPa and reaches 50 GPa. TiAlN can retain high-temperature hardness around 900 to 1000 °C through spinodal decomposition. In dry milling of Hadfield steel, CVD TiCN/Al₂O₃ inserts outperformed PVD TiAlN inserts in one cited study. Texture combined with TiN-WS₂ reduced friction and adhesive wear in dry machining.
Geometry must match material brittleness
Section titled “Geometry must match material brittleness”Positive rake angles lower cutting forces and heat, but may weaken brittle edges. Negative rake angles place the cutting edge in compression and improve chipping resistance during hard turning. Clearance angle controls rubbing and edge support. Too little clearance raises flank wear, while excessive clearance reduces edge strength. Edge honing spreads load across the cutting edge and reduces stress concentration. Excessive rounding can raise ploughing forces and energy use. For PCD, the review calls for sharp edges in non-ferrous work and reinforced edges for composites. Chip breakers control chip curl and evacuation, which controls heat and built-up edge. Tool-life models should therefore combine material properties with cutting geometry.
Selection by operation
Section titled “Selection by operation”For conventional steel turning at 150 to 350 m/min, multilayer TiAlN and AlCrN coated carbides offer a balance of properties. For hardened steels above 45 HRC, the review favors PCBN because of hot hardness and chemical stability. General milling favors coated carbides, while high-speed milling of hardened materials favors fine-grained PCBN or nanocomposite-coated carbides. Ceramics can run at 2 to 3 times the cutting speed of cemented carbides, but their brittleness limits interrupted cutting. Si₃N₄-based ceramics and AlCrN-coated carbides suit nickel-based superalloys. PCD targets aluminium, copper, fibre-reinforced composites, ceramics, and glass. The review reports application speeds up to 3000 m/min for non-ferrous alloys and composites. In one Ti-6Al-4V milling study above 100 m/min, PCD lasted longer than coated carbide. That result does not remove PCD’s chemical limitation in ferrous work.
Limits and unresolved issues
Section titled “Limits and unresolved issues”No material combines maximum hardness, toughness, chemical stability, low friction, and low cost. HSS has limited hot hardness, while ceramics have low fracture toughness. Within WC-Co, more cobalt improves toughness but reduces hardness and high-temperature strength as the binder softens. Refining WC grains improves hardness and abrasion resistance through grain-boundary strengthening. PCD and CBN remain brittle, and their use is selective because of cost and application requirements. CBN, Sialon, and whisker-reinforced ceramic tools cost more than 10 times commercially coated cemented carbides. The review’s tables combine results from different studies rather than one normalized test program. Additively made tools may also contain porosity, residual tensile stress, and columnar anisotropy. Sensor-integrated tools and AI selection remain emerging rather than established industrial practice. Process planning must therefore match the workpiece, cutting conditions, geometry, and production economics.
Materials and support
Section titled “Materials and support”Polycrystalline diamond is the relevant material family for the review’s PCD cutting tools in non-ferrous alloys, composites, ceramics, and glass. These tools need a hard, low-friction layer, sometimes bonded to a tougher WC substrate, with edge geometry matched to load continuity. The 6CCVD diamond materials catalog lists MPCVD-grown polycrystalline diamond plates and wafers; use engineering support to assess these stock forms against a specified tool design.
View Original Abstract
Cutting tool material selection plays an influential role in the performance, precision, and economic viability of metal-cutting operations. This article presents a comprehensive review of current and emerging cutting tool materials, examining their properties, applications, and limitations. The discussion covers widely used options such as high-speed steels, ceramics, cemented carbides, cermets, polycrystalline diamond (PCD), and cubic boron nitride (CBN), along with promising next-generation materials. Emphasis is placed on key performance attributes, including hardness, wear resistance, thermal conductivity, and fracture toughness, which directly influence tool life, surface quality, and machining productivity. Developments in surface engineering, particularly in physical vapour deposition (PVD), chemical vapour deposition (CVD), and advanced nano-composite coatings, are also addressed, highlighting their role in enhancing tool performance under challenging cutting conditions. By reviewing machining studies across different alloys, the work identifies persistent challenges, including tool degradation at high cutting speeds, processing of hard-to-machine materials, and cost optimization. The review concludes by outlining future directions for material innovation to improve efficiency, sustainability, and competitiveness in modern manufacturing. An integrated review of cutting tool materials, surface engineering, wear mechanisms, cost considerations, and intelligent tools is presented. The review further presents a mechanistic analysis of abrasive, adhesive, diffusion, and oxidative wear, linking tool composition and coating architecture to degradation behaviour under extreme machining conditions.
Diamond Heat Spreader With Copper Coated Metalized Surface