Skip to content

Emergence of superconductivity in Th3P4-type Sn3Se4 and Ge3S4 under high pressure synthesized by diamond anvil cell with boron-doped diamond electrodes

FieldValue
JournalFigshare
Published2026-07-23
AuthorsRyo Matsumoto, Satoshi Nakano, Kensei Terashima, Toru Shinmei, Tetsuo Irifune
DOI10.6084/m9.figshare.33071740.v1

The measurements found superconducting transitions in Th3P4-type Sn3Se4 at 8, 12, 15, 19, and 23 GPa. Transitions were also found in Ge3S4 at 11, 16, 22, 27, and 30 GPa. The highest onset temperature was 10.4 K for Ge3S4 at 11 GPa. The largest reported zero-temperature upper critical field was 12.4 T at the same pressure.

Pressure-dependent superconducting transitions

Section titled “Pressure-dependent superconducting transitions”

Table S1 reports transition temperatures determined with the onset criterion. For Sn3Se4, the onset was 7.9 K at 8 GPa. It decreased to 7.1 K at 12 GPa, 6.1 K at 15 GPa, 4.9 K at 19 GPa, and 4.3 K at 23 GPa.

For Ge3S4, the onset was 10.4 K at 11 GPa. It decreased to 9.9 K at 16 GPa, 8.5 K at 22 GPa, 7.8 K at 27 GPa, and 6.8 K at 30 GPa.

MaterialPressure (GPa)Tconset (K)μ0Hc2(0) (T)
Sn3Se487.94.4
Sn3Se4127.14.1
Sn3Se4156.12.6
Sn3Se4194.9Not reported
Sn3Se4234.31.8
Ge3S41110.412.4
Ge3S4169.97.6
Ge3S4228.55.6
Ge3S4277.85.1
Ge3S4306.84.7

Both compounds showed a lower onset temperature as pressure increased over their measured points. The pressure grids differ, so the maxima do not provide a matched-pressure comparison between the materials. The supplied supplement also gives no prior-study benchmark for judging either value against previous work.

Resistance measurements and transition criteria

Section titled “Resistance measurements and transition criteria”

Electrical resistance was recorded over the full temperature region under each pressure. The authors determined Tc using onset, middle, and zero criteria in Figure S3. Figure S4 plots each criterion against pressure and the transition width, defined as Tconset minus Tczero.

Table S1 lists only the onset values. It does not provide numerical middle or zero temperatures or individual transition widths. The reported onset should therefore not be presented as a zero-resistance temperature. The missing values also prevent a direct numerical comparison of transition sharpness between Sn3Se4 and Ge3S4.

The full resistance-temperature curves are shown in the supplemental resistance figure. They provide the measurement context for the tabulated onset temperatures, while the separate field figure plots the temperature dependence of μ0Hc2 under several pressures.

The tabulated zero-temperature upper critical field also fell as pressure rose. For Sn3Se4, μ0Hc2(0) changed from 4.4 T at 8 GPa to 4.1 T at 12 GPa and 2.6 T at 15 GPa. It reached 1.8 T at 23 GPa, while the 19 GPa entry is not reported.

For Ge3S4, μ0Hc2(0) was 12.4 T at 11 GPa. It decreased to 7.6 T at 16 GPa, 5.6 T at 22 GPa, 5.1 T at 27 GPa, and 4.7 T at 30 GPa.

The Ge3S4 value at 11 GPa is the strongest field result in the data. It is larger than the Sn3Se4 maximum of 4.4 T, but each value was measured at a different pressure. The supplied text gives no fitting uncertainty, field orientation, or sample-to-sample spread.

Among the reported values, onset temperature and upper critical field move in the same direction within each compound. Both quantities decline as pressure increases. These trends apply only to the tabulated pressure points and do not establish how the superconductors behave outside the measured ranges.

Sn3Se4 and Ge3S4 were synthesized under high pressure in a diamond anvil cell fitted with boron-doped diamond electrodes. After synthesis, the authors performed LeBail refinement for both compounds. Figure S1 shows typical fitting results for Sn3Se4 and Ge3S4.

Figure S2 tracks the ratio of peak intensity for each phase during Sn3Se4 synthesis as pressure changed. The supplied caption does not identify the phases or list the ratios. The figure is therefore limited to a relative comparison of the diffraction peaks shown in the paper.

The authors also fitted a third-order Birch-Murnaghan equation of state to the two compounds. Figure S5 examines how the fitted B0 and V0 values depend on B0’. No numerical equation-of-state parameters or fit residuals appear in the supplied tables and captions.

The supplemental text gives no numerical lattice constants, unit-cell volumes, or phase fractions. It also provides no counterpart to the Sn3Se4 phase-ratio plot for Ge3S4. Quantitative comparison of phase evolution and compressibility would require data beyond those presented here.

Pressure was calibrated with different markers for the two compounds. Sn3Se4 used the ruby fluorescence peak, while Ge3S4 used the diamond Raman peak. Table S2 records the cell stroke, marker wavelength, and pressure for each calibration point.

MaterialPressure markerStroke (μm)Marker wavelength (nm)Pressure (GPa)
Sn3Se4Ruby fluorescence peak0702.523
Sn3Se4Ruby fluorescence peak−40701.2519
Sn3Se4Ruby fluorescence peak−60699.715
Sn3Se4Ruby fluorescence peak−70698.612
Sn3Se4Ruby fluorescence peak−80697.18
Sn3Se4Ruby fluorescence peak−90695.94
Ge3S4Diamond Raman peak0139930
Ge3S4Diamond Raman peak−40139427
Ge3S4Diamond Raman peak−50138222
Ge3S4Diamond Raman peak−60136916
Ge3S4Diamond Raman peak−70135911

For Sn3Se4, the ruby peak shifted from 702.5 nm at 23 GPa to 695.9 nm at 4 GPa. For Ge3S4, the diamond Raman peak shifted from 1399 nm at 30 GPa to 1359 nm at 11 GPa. The 4 GPa Sn3Se4 calibration point has no corresponding transition or upper-critical-field entry in Table S1.

The calibration ranges overlap, but the compounds share no identical tabulated superconducting pressure. A cross-compound comparison therefore combines material identity with a different pressure schedule and marker system.

Engineering implications and evidence limits

Section titled “Engineering implications and evidence limits”

The paper identifies boron-doped diamond as the electrode material in the diamond anvil cell. That setup supported high-pressure synthesis and in situ electrical resistance measurements at pressures up to 30 GPa. For Ge3S4, the pressure measurement also relied on a diamond Raman peak.

A cell designed to repeat this work must account for both electrical contact requirements and a trackable Raman pressure reference. The supplemental material does not evaluate alternative electrode materials or report electrode dimensions and contact resistance. It therefore cannot establish whether another electrode design would improve the measurement or extend the pressure range.

Material comparisons should retain both the applied pressure and the Tc criterion. Onset values cannot be treated as zero-resistance temperatures. The supplied text also omits starting material preparation, sample geometry, pressure uncertainty, phase fractions, and transition uncertainties. It contains no superconducting measurement below the tabulated ranges. The results support boron-doped diamond electrodes as the configuration used in this study, but they do not define their performance limits.

The paper’s diamond anvil cell uses boron-doped diamond electrodes for high-pressure synthesis at pressures up to 30 GPa. 6CCVD’s diamond materials catalog lists boron-doped diamond and metallization with Au, Pt, Pd, Ti, W, or Cu for contact designs. The engineering support service can be used to define candidate electrode geometry and a metallized contact stack for the cell.

View Original Abstract

High-pressure techniques provide a powerful approach for exploring superconducting materials by enabling structural modifications that significantly alter electronic and phonon properties. In this study, we investigate the emergence of superconductivity in Sn<sub>3</sub>Se<sub>4</sub> and Ge<sub>3</sub>S<sub>4</sub> with the Th<sub>3</sub>P<sub>4</sub>-type cubic structure using high-pressure synthesis and in situ electrical transport measurements in a diamond anvil cell equipped with boron-doped diamond electrodes. Both compounds exhibit superconductivity, with maximum transition temperature <i>T</i><sub>c</sub> of 7.9 K at 8 GPa for Sn<sub>3</sub>Se<sub>4</sub> and 10.5 K at 11 GPa for Ge<sub>3</sub>S<sub>4</sub>. The behavior of the <i>T</i><sub>c</sub> as a function of pressure and previously reported theoretical calculations, including related compounds, suggest a phonon-mediated BCS-type mechanism for observed superconductivity. These results expand the family of Th<sub>3</sub>P<sub>4</sub>-type superconductors and demonstrate the effectiveness of high-pressure techniques for discovering new superconducting phases. Sn<sub>3</sub>Se<sub>4</sub> and Ge<sub>3</sub>S<sub>4</sub> are synthesized at high pressure, and superconductivity in both compounds has been reported for the first time.