Silicon-MediatedLaser Shock Synthesis of NanocrystallineDiamonds from Low-Rank Coal
Paper details
Section titled “Paper details”| Field | Value |
|---|---|
| Journal | Figshare |
| Published | 2026-07-08 |
| Authors | Yanmei Zhang (122913), Zhenghe Zhang (1785097), Rui Wang (52434), Zheng He, Z H Wei |
| DOI | 10.1021/acsnano.6c05022.s001 |
The study reports a synthesis rate of about 18.3 mg/hr for converting low-rank long-flame coal into nanocrystalline diamond. Each production run took about 55.2 s, and the reported crystal size was about 5 nm. High-resolution transmission electron microscopy and selected-area electron diffraction support the diamond assignment. The experiments compare coal with silicon and silicon carbide additives.
Production rate and time accounting
Section titled “Production rate and time accounting”The production rate was calculated from the mass increase of a filtered, purified nanocrystalline diamond-loaded membrane. Original membranes weighed 63.7 mg to 64.8 mg. Loaded membranes weighed 64.0 mg to 65.2 mg. The measured mass gains were 0.4 mg, 0.3 mg, 0.1 mg, 0.3 mg, and 0.3 mg.
The corresponding production rates were 26.1, 19.6, 6.5, 19.6, and 19.6 mg/hr. Together, these values give the reported rate of about 18.3 mg/hr. Sample 3 produced 0.1 mg and had the lowest rate, at 6.5 mg/hr. The other four samples produced 0.3 mg to 0.4 mg each. Their rates ranged from 19.6 mg/hr to 26.1 mg/hr.
This calculation applies to membrane mass gain rather than the mass of coal converted. The reported rate therefore measures recovered nanocrystalline diamond on the filter membrane.
Coal composition and silicon-containing precursors
Section titled “Coal composition and silicon-containing precursors”The starting long-flame coal was purified before use. Its measured composition was 74.14 wt % carbon, 4.51 wt % hydrogen, 0.98 wt % nitrogen, 0.31 wt % sulfur, and 20.06 wt % other elements. Joule heating removed most of the hydrogen. After dehydrogenation, the coal contained 93.76 wt % carbon, 0.60 wt % hydrogen, 1.23 wt % nitrogen, 0.27 wt % sulfur, and 4.14 wt % other elements. HRTEM and selected-area electron diffraction were used to characterize the dehydrogenated coal.
The shock experiments used coal pellets containing silicon or silicon carbide. Products from pure coal pellets served as the no-additive case. The supplemental figures include a C 1s XPS spectrum for coal/Si before laser shock. They also include XRD patterns from the coal/SiC surface before and after irradiation. PL spectra were collected from coal/SiC products and from products synthesized from a single long-flame coal specimen.
Molecular models compared coal without additives, coal with silicon, and coal with silicon carbide. The analysis used the first interfacial coal layer as the center region for C-C radial distribution functions. It also calculated C-C-C bond-angle distributions.
The reference values were 109.5° for diamond-like tetrahedral carbon and 120° for graphitic sp2 carbon. These markers provide a basis for examining local carbon coordination during shock treatment. The supporting information does not extract a numerical diamond phase fraction from the simulated distributions.
Laser shock conditions and pressure estimates
Section titled “Laser shock conditions and pressure estimates”An infrared monochromatic pyrometer monitored the IRco laser process. Thermal accumulation occurred over 5 s to 15 s, and the measured peak temperature was about 765 K. The IRco experiment used coal/SiC pellets dispersed in water. Products from coal/SiC, coal/Si, and pure coal pellets were also characterized under the pulsed IRps process.
The authors estimated peak pressure with the Fabbro model instead of measuring interface pressure directly. The calculated nominal peaks were about 15.7 GPa for IRps and 114.9 GPa for IRfs. The authors state that these values are not actual interfacial pressures.
The model used a coupling efficiency, alpha, of 0.1. This conservative value accounts for possible energy loss from nonlinear absorption and plasma shielding in the water layer. Shock impedance combined the specimen and water values. The specimen was approximated by graphite at 7.5 × 10^5 g·cm^-2·s^-1. Water was set at 1.65 × 10^5 g·cm^-2·s^-1.
The calculation also uses laser intensity, pulse energy, pulse width, and laser spot area. Their values are not supplied in the supporting information. This prevents reproduction of the pressure estimates from the reported excerpt alone.
Diamond identification and optical characterization
Section titled “Diamond identification and optical characterization”SAED rings were indexed with the D(111), D(220), and D(311) reflections of cubic diamond. The measured spacings closely followed the standard values in both IRco and IRps products.
| Reflection | Standard cubic diamond, d (nm) | IRco product, measured d (nm) | IRps product, measured d (nm) |
|---|---|---|---|
| D(111) | 0.206 | 0.20 | 0.21 |
| D(220) | 0.126 | 0.13 | 0.13 |
| D(311) | 0.107 | 0.11 | 0.11 |
HRTEM supplied particle images of the synthesized material. Table S5 assigns the product a crystal size of about 5 nm. PL spectra were collected under excitation at 240, 245, and 250 nm. The supporting text does not give numerical emission peaks or luminescence yield.
XPS and XRD provide complementary chemical and phase measurements on selected pellets. In the IRps coal/SiC sample, the diffraction pattern marks both diamond and silicon carbide crystals. The characterization therefore establishes the presence of diamond without demonstrating phase-pure diamond material.
Comparison with other coal conversion routes
Section titled “Comparison with other coal conversion routes”Table S5 places the shock process among six earlier coal conversion methods. The comparison includes low-rank and high-rank coal, so it does not isolate precursor rank from process effects.
| Method | Precursor | Crystal size | Synthesis rate | Synthesis time |
|---|---|---|---|---|
| Laser ablation | High-rank coal | ~3 nm | 0.125 to 0.250 mg/hr | n/a |
| Hydrogenation and acid/alkali treatment | High-rank coal | ~35 nm | n/a | 24 h |
| Oxidation treatment | Low-rank coal | ~2 nm | n/a | 9 h |
| Acidic oxidation and ultrasound | Low-rank coal | ~4 nm | n/a | 2 h |
| Ultrasonic-assisted stimulation in hydrogen peroxide | Low-rank coal | 4 to 15 nm | n/a | 3 h |
| Electron beam irradiation | High-rank coal | 2 to 10 nm | n/a | 30 s |
| Laser-induced shockwave, this work | Low-rank coal | ~5 nm | ~18.3 mg/hr | ~55.2 s |
The shock method has the highest listed synthesis rate in Table S5. The laser ablation rate is 0.125 to 0.250 mg/hr for a crystal size of about 3 nm. The oxidation, acidic oxidation with ultrasound, and peroxide-assisted routes list synthesis times of 9 h, 2 h, and 3 h, respectively.
The electron beam method lists a processing time of 30 s but provides no synthesis rate. The shock process took about 55.2 s per sample. Its rate was calculated from membrane mass increase, while Table S5 does not state the production basis for the laser ablation rate. The comparison supports a processing-time distinction but does not provide a complete rate comparison for every method.
Engineering interpretation and unresolved limits
Section titled “Engineering interpretation and unresolved limits”The reported output is a purified membrane carrying diamond particles with a reported size of about 5 nm. The paper does not report a bulk diamond plate or wafer. For material selection, the process supports a particulate diamond route. The PL measurements provide optical characterization under 240 nm to 250 nm excitation, but they do not establish device-level optical performance.
The pressure values remain model estimates rather than direct interface measurements. The five measured production rates range from 6.5 mg/hr to 26.1 mg/hr. Silicon carbide was also identified beside diamond in the coal/SiC product.
The supplied information does not report particle size distribution, diamond phase fraction, chemical purity, or electrical, thermal, and mechanical properties. Those measurements are needed before assigning the material to a specific device function. The immediate engineering result is a rapid route to nanoscale particulate diamond, not qualification data for a monolithic diamond component.
View Original Abstract
Coal is traditionally regarded as a primary energy resource for combustion. However, its high carbon content renders it an ideal precursor for the synthesis of carbon nanomaterials. The valorization of low-value coal into high-value nanocrystalline diamonds (NDs) offers a promising strategy. In this work, we developed a facile and rapid strategy for the synthesis of NDs from low-rank long-flame coal via silicon-mediated laser-induced shockwave high pressure within a water-confinement layer. The as-synthesized products show an average crystallite size of ∼5 nm and exhibit features consistent with cubic diamond, including the (111), (220), and (311) reflections and ∼0.20 nm lattice fringes with a ∼70° intersection angle. C 1s X-ray photoelectron spectroscopy indicates an enhanced sp<sup>3</sup>-bonded carbon contribution after laser shock treatment. Raman spectra of the coal/Si pellet surfaces demonstrate that the laser-induced coal-to-ND transformation is a kinetically controlled process. Molecular dynamics (MD) simulations reveal that the chemical reaction between coal-derived carbon and active Si additives may locally provide an additional chemical driving force, which promotes C-C bond activation and accelerates the formation of sp<sup>3</sup>-like, diamond-like structural motifs. These findings provide a sustainable route for the synthesis of NDs from abundant and inexpensive coal, advancing the clean and high-value-added utilization of coal resources.
Single Crystal Cvd Diamond Plate
View Specs →
Boron Doped Single Crystal Diamond Plate
View Specs →