Synergistic boron-doped diamond/polyaniline/SnO2 nanoparticle- screen-printed electrode for electrochemical detection of chloramphenicol
Paper details
Section titled “Paper details”| Field | Value |
|---|---|
| Journal | Results in Chemistry |
| Published | 2026-09-21 |
| Authors | Indi Anfita Afany, Bintang Adji Notodidjojo, Prastika Krisma Jiwanti, Mai Tomisaki, Wan Jefrey Basirun |
| DOI | 10.1016/j.rechem.2026.103892 |
A boron-doped diamond/polyaniline/SnO2 nanoparticle-modified screen-printed electrode detected chloramphenicol over 1 to 100 µM at pH 7.0. It had a 0.49 µM limit of detection and a 1.63 µM limit of quantification. Peak-current response showed a 0.59% RSD across seven separately prepared electrodes measured on different days. Spiked tablet, milk, and chicken meat samples gave recoveries of 104.05%, 101.36%, and 91.78%, respectively.
Analytical performance
Section titled “Analytical performance”Chloramphenicol standards of 0, 1, 10, 20, 40, 60, 80, and 100 µM were measured by differential pulse voltammetry in phosphate buffer at pH 7.0. Each concentration was measured in triplicate, and the calibration had R² > 0.995. The potential range was −1.0 to 1.5 V versus Ag/AgCl. The settings included a 0.012 V step, a 0.1 V pulse, and a 6 mV/s scan rate. The signal was the DPV peak current at the characteristic chloramphenicol potential.
LOD and LOQ used the standard deviation of three blank measurements and the calibration slope. Selectivity was tested with D-glucose, ciprofloxacin, levofloxacin, ascorbic acid, and NaCl at 100 µM. Current changes were 3.15%, 2.80%, 2.96%, 3.06%, and 3.00%, respectively. These results cover only the five tested interferents.
Electrode fabrication
Section titled “Electrode fabrication”SnO2 nanoparticles were prepared by a sol-gel route. The authors dissolved 3.3 g of SnCl2·2H2O in 30 mL ethanol and stirred for 60 min. They added 1 M NH3 until pH 8. The washed precipitate was dried at 90 °C for 3 h and calcined at 500 °C for 2 h.
The PANI@SnO2NP composite was formed by in situ oxidative polymerization. They placed 0.8 mL of 1 M aniline in 10 mL of 1 M HCl and stirred for 30 min at 0 to 5 °C. They added 0.15 g SnO2NP and ultrasonicated for 30 min. They then added 2.28 g ammonium persulfate in 10 mL HCl dropwise under stirring for 3.5 h. The washed composite was dried at 60 °C for 12 h.
For coating, the authors made BDD ink with 30% ethanol and sonicated it for 1 h. They drop-cast 6 µL of ink onto a screen-printed electrode and dried it at 50 °C for 30 min. They then added 6 µL of PANI@SnO2NP solution and repeated the drying step. The paper omits the BDD concentration in the ink.
Composite structure
Section titled “Composite structure”XRD identified PANI and tetragonal rutile SnO2 in the composite. The SnO2 nanoparticles had an average crystallite size of 13.33 nm, while TEM measured an average particle size of 22.65 nm. SEM showed agglomerated PANI particles averaging 600 nm. The composite had a more defined fibrous morphology, with an average PANI width of 63 nm and SnO2NP domains along the fibers.
UV-Vis showed the SnO2 peak shifting from 292 nm to 298 nm after PANI incorporation. The authors interpret this as electronic coupling between PANI and SnO2NP. FTIR detected characteristic PANI and Sn-O-Sn bands without substantial shifts. These results support incorporation of both phases but do not quantify their separate electron-transfer contributions during detection.
Electrochemical response
Section titled “Electrochemical response”Cyclic voltammetry in 0.1 M KCl with 5 mM potassium ferricyanide gave an electrochemically active area of 0.012 cm² for SPE/BDD. It was 0.12 cm² for SPE/PANI, 0.41 cm² for SPE/PANI@SnO2NP, and 0.38 cm² for SPE/BDD/PANI@SnO2NP. The authors suggest that the BDD layer partly limited access to the composite surface.
At 100 µM chloramphenicol in pH 7 buffer, the full electrode had the highest signal-to-background ratio. Its S/B value was 2.87, compared with 2.09 for SPE/BDD, 2.13 for SPE/PANI, and 2.17 for SPE/PANI@SnO2NP. The full electrode had less active area but higher S/B, so active area alone did not determine sensitivity.
The proposed mechanism starts with reduction of chloramphenicol to hydroxylamine chloramphenicol during the negative scan. The positive scan oxidizes that product to a nitroso derivative near 0 V, and the oxidation response is the analytical signal. The authors attribute the response to BDD stability, low background current, and a wide potential window, plus conductive PANI and active SnO2NP sites.
Comparison with prior sensors
Section titled “Comparison with prior sensors”The full electrode did not set the lowest reported LOD. A MoS2/MWCNT glassy carbon electrode gave 0.4 µM over 1 to 35 µM. A Fe3O4@MXene@Fe-BDC screen-printed electrode gave 0.26 µM over 1 to 309 µM. Two AuNP-modified screen-printed electrodes gave 0.1 and 0.66 µM over 0.25 to 50 µM. The introduction also cites PANI nanorods/RGO at 1 nM.
| Electrode | Concentration range | LOD | Reproducibility |
|---|---|---|---|
| GCE/MoS2/MWCNT | 1 to 35 µM | 0.4 µM | 2.92% RSD |
| GCE/Co3O4@rGO | 0.1 to 50 µM | 1.16 µM | 1.7% RSD |
| SPE/Fe3O4@MXene@Fe-BDC | 1 to 309 µM | 0.26 µM | 1.23% RSD |
| SPCE/AuNP | 0.25 to 50 µM | 0.1 µM | Not reported |
| SPPtE/AuNP | 0.25 to 50 µM | 0.66 µM | Not reported |
| SPE/BDD/PANI@SnO2NP | 1 to 100 µM | 0.49 µM | 0.59% RSD |
The new sensor’s 0.59% RSD was below every reported prior RSD. Its disposable format differs from the drop-cast glassy carbon electrodes and standalone cells in many cited studies.
Food matrix recovery
Section titled “Food matrix recovery”One milliliter of milk was mixed with 5 mL of 0.1 M PBS, vortexed, centrifuged for 5 min, and filtered. A 3 g chicken sample was homogenized in 10 mL PBS, ultrasonicated for 30 min, centrifuged at 4000 rpm for 5 min, and filtered. A 250 mg chloramphenicol tablet was dissolved in 747 mL PBS and diluted tenfold before spiking. Each measurement used 10 µL of extract and three replicates.
The tablet peak current increased by 34.14 µA after spiking. Milk and chicken signals reached 33.74 µA and 32.27 µA, respectively. Milk and chicken produced more background current than buffer. The tablet blank had a broad minor peak that the authors say may reflect trace chloramphenicol.
| Matrix | Spiked concentration | Obtained concentration | Recovery | RSD |
|---|---|---|---|---|
| Tablet | 100 µM | 104.049 µM | 104.049% | 0.202% |
| Milk | 100 µM | 101.360 µM | 101.360% | 0.521% |
| Chicken meat | 100 µM | 91.776 µM | 91.776% | 0.018% |
These results cover one 100 µM spike level. They do not establish performance across native contamination levels or against a reference chromatographic method.
Remaining validation and design limits
Section titled “Remaining validation and design limits”Further development and testing are required before practical deployment. The authors call for validation against established analytical methods and standardized instruments. They also identify wider interferent testing, operational stability, and storage stability as unresolved. Lower-concentration detection remains a design target. Proposed routes include nanotubular PANI, direct incorporation of BDD and tin oxide into PANI, and morphology changes that increase accessible surface area.
Several reported details need care. The abstract gives a maximum selectivity deviation of 3.06%, while the body gives a 3.15% change for D-glucose. The LOD and LOQ use three blank measurements. Real-sample recovery uses one 100 µM spiking level, and the paper omits the BDD ink concentration. The reproducibility spectra also retained a peak near +0.5 V that the authors assigned to residual potassium ferricyanide.
For sensor engineering, the active-area and S/B comparison is the main design lesson. BDD supplied a stable, low-background platform, while PANI@SnO2NP supplied the conductive active interface. Removing BDD increased ECSA but lowered S/B here. The data support the full layer sequence for this assay, not a universal rule for chloramphenicol sensors.
Materials and support
Section titled “Materials and support”For a screen-printed chloramphenicol sensor, the relevant material family is boron-doped diamond. The paper used BDD powder dispersed in 30% ethanol as printable ink, while 6CCVD’s diamond materials catalog lists boron-doped diamond as the matching material. The feedstock form still needs confirmation, and engineering support can address the 6 µL BDD coating and its integration with PANI@SnO2NP.
View Original Abstract
Chloramphenicol (CAP) in food products pose serious health risks, requiring rapid and rapid and reliable methods for on-site monitoring. Herein, a portable electrochemical sensor based on boron doped diamond (BDD) and polyaniline/tin oxide nanoparticles (PANI@SnO 2 NP)-modified screen-printed electrode (SPE) was developed for CAP detection. PANI@SnO 2 NP was prepared through in-situ oxidative polymerization. Structural and morphological characterizations were characterized using UV-Vis, FTIR, XRD, SEM-EDX, and TEM. Electrochemical performances were evaluated using cyclic voltammetry (CV) and differential pulse voltammetry (DPV). SPE/BDD/PANI@SnO 2 NP exhibited a linear response in the range of 1-100 μM, with a limit of detection (LOD) of 0.49 μM and limit of quantification (LOQ) of 1.63 μM. The sensor demonstrated good selectivity with maximum deviation of 3.06%, and excellent reproducibility (%RSD = 0.59%). CAP Recovery values in real samples (tablet, milk, and chicken meat) ranged from 91.78-104.05%. The proposed platform demonstrates potential for portable CAP detection in food safety applications. For future improvements, other shape of PANI can be used for higher surface area.