Experimental investigation of using diamond crystal as a high temperature sensor
Paper details
Section titled “Paper details”| Field | Value |
|---|---|
| Journal | Results in Materials |
| Published | 2026-10-30 |
| Authors | Mostafa Hassanzadeh, Mohsen Asadi Asadabad, Aref Rahimian, Heidar Faripour, Ehsan Boustani |
| DOI | 10.1016/j.rinma.2026.101075 |
A natural diamond irradiated to 2 × 10²⁰ n/cm² became X-ray amorphous, while heat treatments between 600 °C and 800 °C produced weak recovery features. The clearest reported response followed 700 °C annealing, with an integrated intensity about 8% of the pristine (111) peak. Because recovery remained incomplete and most treated samples stayed amorphous, the work identifies a candidate annealing window but not a reliable peak-temperature sensor.
Sensor principle and measurement target
Section titled “Sensor principle and measurement target”Maximum-temperature crystalline sensors use neutron-induced lattice expansion as a stored temperature record. Irradiation creates displacement defects and vacancies, which increase crystal volume. Heating contracts the damaged lattice, so lattice parameters before and after annealing can estimate peak temperature when temperature and exposure time are controlled. The method is intended for post-event peak-temperature measurement rather than continuous monitoring.
The paper cites prior MTCS work that can determine temperature within a few degrees up to 1000 °C and even above 1000 °C. That performance belongs to the prior concept, not to the natural diamond specimen tested here. The cited maximum measurable temperature for diamond is about 900 °C, compared with up to 1400 °C for 3C-SiC.
The experiment did not reconstruct an unknown peak temperature from the specimen. It instead mapped which annealing conditions left a measurable diffraction signal after severe irradiation.
Sample characterization and irradiation
Section titled “Sample characterization and irradiation”The natural diamond weighed 1.601 g. XRF detected mainly Fe, Cu, Zn, and Zr, totaling about 0.86 wt%. This was not a total purity result. Conventional XRF detects elements with atomic number greater than 11, so B, N, O, and H were not detected. The reported apparent purity of 99.14% applies only if the light elements are absent, which the authors say is rarely true for natural diamond.
The specimen was wrapped in 0.5866 g of aluminum foil and placed in an aluminum container 2 cm high and 3 cm in diameter. A buoyancy test preceded placement in channel F8 of compact core No. 18. The target exposure used fast neutrons above 0.18 MeV.
The sample accumulated a fluence of 2 × 10²⁰ n/cm² during 189 days of intermittent operation. Its average fast neutron flux was 3.1 × 10¹³ n/cm²/s, with an average measurement-based error of about 10%. The calculated axial flux for the sample position peaked at 5.01 × 10¹³ n/cm²/s.
Radiation activity and handling
Section titled “Radiation activity and handling”Impurity activation created a radiological handling constraint. Total sample activity fell from 100 µCi to 10 µCi over four months of cooling. At a distance of 1 m, the reported photon dose rate fell from 21 µSv/h to 1.4 µSv/h across the cooling conditions.
An ALNOR gamma dosimeter measured about 5 mSv/h next to the sample after two months of continuous irradiation. The corresponding simulation gave about 4.2 mSv/h, a discrepancy of about 16%. The paper lists aluminum-container activation, model error, location variation, dosimeter error, and reactor operating uncertainty as possible causes.
For transport, the unshielded sample reading was 143 µSv/h. Lead shielding reduced it to 73.7 µSv/h. The authors used that shielding to keep dose rates below permissible limits.
Annealing and characterization methods
Section titled “Annealing and characterization methods”The first screen annealed irradiated diamond at 100, 300, 500, 700, and 900 °C for 90 min. A reference thermocouple beside the specimen kept the sample-temperature error within ±2 °C. The subsequent grid used 50 °C increments between 600 °C and 800 °C.
| Annealing temperature | Annealing times |
|---|---|
| 600 °C | 10, 100, 500 min |
| 650 °C | 10, 100, 500 min |
| 700 °C | 10, 100, 500 min |
| 750 °C | 10, 100, 500 min |
| 800 °C | 10, 100, 500 min |
XRD used Cu Kα radiation with λ = 1.5406 Å, at 40 kV and 30 mA. Data covered 2θ from 20° to 90° in 0.02° steps, with 2 s counting per step. Peaks were fitted with a pseudo-Voigt function in High Score software. Lattice parameters and volumes were derived from detectable peaks using Bragg’s law.
Differential scanning calorimetry used 10 °C/min from 25 °C to 900 °C, with a 40 ml/min flow of 40Ar gas.
Recovery and lattice response
Section titled “Recovery and lattice response”The pristine sample matched ICDD PDF 96-901-1998, with diamond peaks near 44° and 75° in 2θ. The irradiated sample showed no discernible crystalline peaks. The authors describe this as complete structural amorphization within the detection limits of laboratory XRD. The paper reports that annealing at 500 °C or below failed to restore detectable crystallinity.
The highlighted 700 °C treatment produced a weak peak at 74.98° ± 0.05° in 2θ. Its FWHM was 0.42° ± 0.08°. The broad feature indicated partial recovery with residual disorder. A DSC heat-flow anomaly near 650 °C resembled an exothermic crystallization feature. The authors treated this assignment as tentative because the test lacked in situ XRD and higher-resolution thermal analysis.
Most samples in the annealing grid still produced no identifiable crystalline peaks. The lattice entries reported in the paper were:
| Sample | Annealing condition | 2θ | Reflection | ΔV/V |
|---|---|---|---|---|
| 70010 | 700 °C for 10 min | 74.6034° | (220) | 0.027689425 |
| 80010 | 800 °C for 10 min | 74.7761° | (220) | 0.021613404 |
| 700100 | 700 °C for 100 min | 43.4154° | (111) | 0.051529032 |
| 750100 | 750 °C for 100 min | 43.4851° | (111) | 0.054546222 |
| 600500 | 600 °C for 500 min | 43.3353° | (111) | 0.059714563 |
The reference pattern placed the (111) reflection at 44.2255° and the (220) reflection at 75.4033°. The listed annealed peaks remained slightly displaced from those references. The reported ΔV/V values are preliminary relative-volume changes, not a validated temperature calibration.
The text says the primary peak near 44° was not recovered in any annealed sample. Table 6 nevertheless lists three (111) entries near 43°. That internal inconsistency must be resolved before these values can support a calibration.
Comparison with prior sensors
Section titled “Comparison with prior sensors”The amorphization result is qualitatively consistent with prior work cited by the authors. Khomich et al. reported complete graphitization in neutron-irradiated diamond above 10²⁰ n/cm². The present specimen received twice that fluence and lost detectable diffraction before annealing. Their suggestion that annealing above 600 °C is needed for defect recombination also agrees with the weak recovery seen here.
The paper cites 3C-SiC as more robust under similar irradiation, with better crystallinity retention and more complete recovery after annealing. The comparison favors 3C-SiC when structural retention is the priority. The paper’s main advance is a preliminary ΔV/V map for natural diamond over a defined annealing grid. Its sparse peaks prevent statistical validation.
Limits and engineering implications
Section titled “Limits and engineering implications”The main limitations are visible in both design and data. Only one natural diamond was irradiated, and it then underwent multiple annealing steps. No replicates or confidence intervals were possible. The fluence of 2 × 10²⁰ n/cm² may have been too high, since most heat-treated states remained X-ray amorphous. Unknown light-element impurities add further variability. The calibration grid also produced few measurable peaks, and the narrative conflicts with the tabulated (111) results.
For sensor development, a candidate must retain a measurable diffraction response after irradiation and annealing. Initial crystallinity alone does not establish that suitability. The authors recommend synthetic high-purity diamond, lower fluences, in situ annealing XRD, and complementary Raman spectroscopy or transmission electron microscopy. The 600-800 °C interval is the justified starting range, with recovery first appearing near 650-700 °C. The next decisive test is a replicated series of synthetic high-purity diamonds irradiated below 2 × 10²⁰ n/cm² and examined by in situ annealing XRD.
View Original Abstract
This paper investigates the feasibility of using diamond in high-temperature environments. These miniaturized sensors made from materials like 3C-SiC, diamond, and graphite exploit the expansion of the crystal lattice due to neutron irradiation, which is then reduced upon heating. Measuring lattice parameters before and after heating allows for accurate temperature determination within a few degrees up to 1000 °C. The study focused on a diamond sensor, calculating fast neutron flux and activity in the Tehran research reactor core. Results showed a significant reduction in diamond activity after approximately 3 months. Pre-and post-irradiation analyses using X-ray fluorescence for impurities and X-ray diffraction (XRD) for phase identification and crystal characteristics were performed. A diamond sample was irradiated for 189 days in the A9 channel of the TRR core to a neutron fluence of 2×1020 n/cm2. Post-irradiation analysis included XRD and thermal analysis to create a calibration curve by heating raw, irradiated, and heat-treated samples at 600-800 °C for 10, 100, and 500 minutes. The results indicate that the diamond crystal lattice returns to its initial state around near the second peak of the reference diamond pattern at 700 °C. Therefore, annealing above 650 °C is suggested for complete lattice recovery when XRD data suggest that the 600-800 °C range is suitable for employing diamond as a high-temperature sensor.
Advanced Thermal Simulation Service Diamond Heat Spreader Performance Analysis
View Specs →
Electronic Grade Intrinsic Diamond Epitaxial Wafer H Terminated Superior 100 Mosfet Ready Substrate