Increasing selectivity of X-ray luminescence separation through the selective fixation of luminophore-containing spectral-kinetic characteristic modifiers on diamonds
Paper details
Section titled “Paper details”| Field | Value |
|---|---|
| Journal | Gornye nauki i tekhnologii = Mining Science and Technology (Russia) |
| Published | 2026-10-22 |
| Authors | V. A. Chanturia, В. В. Морозов, E. L. Chanturia, Самусев Андрей Леонидович, Г. П. Двойченкова |
| DOI | 10.17073/2500-0632-2026-06-1175 |
The authors reported a 15% to 17.5% increase in diamond recovery during X-ray luminescence separation. Their selected treatment used 40 °C, pH 5.5, and 200 mg/L OEDP complexonate. The same regime reduced kimberlite recovery to the concentrate by 0.15% to 0.45%. Selective modifier fixation on kimberlite caused the improvement without pushing treated diamonds outside separator limits.
Why selective fixation controls recovery
Section titled “Why selective fixation controls recovery”Weakly and anomalously luminescent diamonds have spectral-kinetic characteristics unlike the main diamond population. Separators tuned for normally luminescent natural diamonds can therefore lose these crystals. The authors treated them with modifiers containing luminophores and an organic liquid. These composites impart the spectral characteristics expected by the separator.
The treatment required selective fixation because the modifier also collected on hydrophobic kimberlite minerals. This reduced the signal contrast between diamond and kimberlite. Visiometry found 15% to 40% coverage on diamonds and talc, but only 0.5% to 5% on other tested minerals. Kimberlite particle coverage ranged from 0.5% to 25%, with hypergene-altered kimberlite showing the highest values.
Modifier chemistry and test material
Section titled “Modifier chemistry and test material”The collector phase combined heavy catalytic cracking gas oil, diesel technical fraction, and luminol. The MLA-1 formulation used in separation tests contained FL-530 luminophore and a collector made from heavy catalytic cracking gas oil and 15% diesel technical fraction.
The authors tested three regulator classes. Complexonates were OEDP, NTF, and IS-3. The polymer class included Kamtsel 600, CMC-75, and polyethylene glycol 1400. The ethoxylated alkylphenols were Neonol AF-9-6, OP-4, and EO-20.
Model water approximated the composition of circulating water at beneficiation plants. Samples included anomalous-luminescent diamonds, primary and hypergene-altered kimberlite, and polished sections and plates of important minerals.
Measuring surface coverage
Section titled “Measuring surface coverage”Emulsion-treated samples were imaged with a Mikromed 3 LUM microscope and a UFK-254/365 fluorescence cabinet under ultraviolet light. ImageJ 1.54g measured the surface area occupied by collector and luminophore.
The multispectral method distinguished collector emission at 465 nm from luminophore emission at 530 nm. Luminophore occupied 85% to 92% of the total modifier coverage on kimberlite. This confirmed that luminophore remained concentrated within attached collector droplets.
Modifier deposition had a point-like form. It concentrated on talc and muscovite inclusions, with less coverage on calcite and phlogopite. Hypergene-altered kimberlite carried the strongest deposition on massive talc aggregates.
Adhesion energy explains regulator response
Section titled “Adhesion energy explains regulator response”Three-phase contact angles were measured on a DSA25 after conditioning mineral surfaces in the test water. An ST-1 stalagmometer measured interfacial tension from the mass of ten detached droplets. The authors calculated collector adhesion energy with the Dupre-Young equation.
Primary kimberlite had a lower baseline adhesion energy than altered kimberlite, at 7.84 versus 9.92 mJ/m². Across the tested regulator conditions, adhesion fell to 2.16 to 4.86 mJ/m² on primary kimberlite. On altered kimberlite, it fell to 3.33 to 7.29 mJ/m².
Collector adhesion energy at 24 °C and 40 °C. Values are in mJ/m².
| Treatment | Primary at 24 °C | Altered at 24 °C | Primary at 40 °C | Altered at 40 °C |
|---|---|---|---|---|
| No regulator | 7.84 | 9.92 | Not reported | Not reported |
| Complexonates | 4.38 | 5.70 | 4.32 | 4.67 |
| Polymers | 3.12 | 6.12 | 3.01 | 4.91 |
| Ethoxylated alkylphenols | 2.72 | 4.66 | 2.44 | 4.15 |
The paper reports a 3% to 12% adhesion reduction from heating the medium from 24 °C to 40 °C. Contact angles increased while interfacial tension decreased with temperature. The authors linked both trends to the surface-energy balance at the three-phase perimeter.
pH responses depended on the regulator class. From pH 6.7 to 4.5, complexonate adhesion rose from 5.04 to 5.56 mJ/m² on primary kimberlite and from 4.97 to 6.04 mJ/m² on altered kimberlite. Ethoxylated alkylphenol adhesion fell on both types, from 2.69 to 2.47 mJ/m² on primary and 5.22 to 4.50 mJ/m² on altered. Polymer adhesion rose on primary from 3.19 to 4.04 mJ/m² but fell on altered from 6.12 to 5.91 mJ/m². One pH rule therefore does not describe all three regulator classes.
Coverage changes with temperature and pH
Section titled “Coverage changes with temperature and pH”At 20 °C with OEDP, surface coverage was 31.4% on diamonds, 3.5% on primary kimberlite, and 3.8% on altered kimberlite. At 40 °C, these values fell to 28.7%, 1.5%, and 2.2%, respectively.
Heating with OEDP reduced luminophore coverage on kimberlite by a factor of 1.8 to 2.5. The two kimberlite values at 40 °C were below the 3% threshold at which kimberlite can enter the separation concentrate. Acidification produced a smaller coverage reduction than heating.
Earlier work cited by the authors used 20 °C and pH 6.7. It reported a 31% to 86% reduction in coverage on kimberlite minerals after regulator addition. The current work tested whether temperature and pH could improve that suppression.
Spectral response remains within separator limits
Section titled “Spectral response remains within separator limits”The authors measured signal convolution, slow-component intensity, and fast-to-slow amplitude ratio. They also calculated the luminescence decay time constant.
Heating to 40 °C did not materially change the kinetic curve shape. Relative changes in the spectral-kinetic parameters did not exceed 25%. Lowering pH also preserved the curve shape, but reduced the slow-component amplitude at 0.7 to 1 ms. Changes could reach 50% at pH 4.5.
Despite these changes, the modified diamonds remained within the separator’s operating ranges and were diagnosed as diamonds. For MLA-1 without a regulator, pH 5.5 gave a signal convolution of 0.35, an amplitude ratio of 2.4, and a decay constant of 3.4 ms. At pH 4.5, the values were 0.33, 3.2, and 3.1 ms.
Separation performance
Section titled “Separation performance”The Polyus-M separator evaluated the modified material in dynamic mode. The original charge combined diamond-free second-stage tailings with 20 diamonds from the minus 3 mm to plus 1.5 mm size class.
Dynamic separation results with MLA-1 and OEDP. Extraction values are percent.
| Treatment | Diamonds at 20 °C | Diamonds at 40 °C | Kimberlite at 20 °C | Kimberlite at 40 °C |
|---|---|---|---|---|
| No modifier | 20.0 | 20.0 | 1.22 | 1.12 |
| MLA-1 without regulator | 75.0 | 87.5 | 1.65 | 1.20 |
| MLA-1 with OEDP, 200 mg/L | 90.0 | 92.5 | 1.16 | 1.00 |
At pH 5.5 with OEDP, extraction was 92.5% for diamonds and 1.01% for kimberlite. At pH 4.5, the values were 90% and 1.26%. At pH 7.2, they were 90% and 1.16%.
Acidification without a regulator increased diamond extraction from 75% at pH 7.2 to 85% at pH 5.5. Kimberlite extraction also rose from 1.65% to 1.90%. The combined OEDP treatment therefore controlled the kimberlite response that acidification alone increased. The reported efficiency coefficient reached 87.5% at 40 °C and 87.3% at pH 5.5.
Engineering implications and unresolved questions
Section titled “Engineering implications and unresolved questions”The result defines a pretreatment step before X-ray luminescence separation. The authors expect lower losses of weakly and anomalously luminescent diamonds. They also expect less kimberlite in rough diamond concentrates, which should reduce costs during finishing operations.
The separation evidence remains based on laboratory tests with 20 added diamonds. The paper reports no replicate count, uncertainty intervals, continuous plant campaign, modifier recovery, or scale-up data. Feed-specific validation is therefore needed before applying the treatment to another kimberlite deposit.
Reproduction also requires resolving two reporting differences. The regulator list names polyethylene glycol 1400, while the spectral-kinetic tables identify PEG 1500. The text states that temperature did not affect complexonate adhesion, while the adhesion table records numerical changes.
The paper’s selected operating point is 40 °C, pH 5.5, and 200 mg/L OEDP before X-ray luminescence separation. Feed checks remain necessary because primary and hypergene-altered kimberlite had different adhesion energies and coating responses.
View Original Abstract
The relevance of the study is determined by the importance of the problem of increasing the efficiency of the X-ray luminescence separation for weakly and anomalously luminescent diamonds, achieved through the selective fixation of luminophore-containing modifying agents (modifiers) on the diamond surface, which are a composition of luminophores and an organic liquid that impart the spectral characteristics of natural diamond to these diamonds. The aim of the research was to increase the selectivity of extracting anomalously luminescent diamonds by selecting medium parameters, primarily the temperature and pH of the aqueous phase, which ensure the selectivity of the fixation of luminophore-containing modifying agents on the surface of diamonds and kimberlite. The study employed methods for measuring limiting wetting angles and surface tension in the mineral-organic collector-aqueous phase system. The Dupré-Young equation was used to calculate the adhesion energy of the apolar collector on the mineral surface. To evaluate the efficiency of organic collector fixation on mineral samples, a visiometric technique was used, which involved obtaining and analyzing images of the mineral surface using a Mikromed 3 LUM microscope and in a UFK-254/365 fluorescence cabinet under ultraviolet light. The research results showed that the modifying agent was fixed and concentrated on inclusions of hydrophobic kimberlite minerals. The proportion of the kimberlite particle surface covered by luminophores after treatment with modifiers ranges from 0.5 to 25%, with the most intensive fixation of luminophores (maximum degree of surface coverage) observed on the surface of hypergene-altered kimberlite. The research findings demonstrated the feasibility of increasing the selectivity of modifying agent fixation on diamond crystals by using various classes of regulating agents: complexonates (OEDP, ATMPA, AQUA-IS-3), organic polymers (Kamtsel-600 (sodium carboxy-methylcellulose), CMC-75, polyethylene glycol 1400), and ethoxylated alkylphenols (Neonol AF-9-6, OP-4, EO-20). It was established that increasing the temperature and decreasing the pH of the medium with the addition of regulating agents of the selected classes is an effective factor that reduces the adhesion energy of the organic collector on the surface of altered kimberlite that ensures decreasing the fixation of a modifying agent on kimberlite particles and, accordingly, contributes to an increase in the selectivity of modifying agent fixation on diamond crystals. Verification of the developed treatment regime for diamond-kimberlite products with spectral-kinetic characteristic modifiers demonstrated its effectiveness. It was shown that by heating the medium to 40 ℃ and acidifying the medium to pH = 5.5 with the addition of OEDP complexonate as a regulating agent to the aqueous phase at a concentration of 200 mg/L, an increase in diamond recovery in the X-ray luminescence separation process by 15-17.5% and a decrease in kimberlite yield into the concentrate by 0.15-0.45% are achieved.
Advanced Thermal Simulation Service Diamond Heat Spreader Performance Analysis
View Specs →Cvd Diamond Coating On Silicon Wafer
View Specs →