Thermal modification of diamond nanoparticles obtained by grinding natural raw materials and detonation synthesis. Part 1. Morphology and structure of nanodiamonds
Paper details
Section titled “Paper details”| Field | Value |
|---|---|
| Journal | Powder Metallurgy аnd Functional Coatings |
| Published | 2026-10-20 |
| Authors | M. P. Akimova, Петр Петрович Шарин, Sofia P. Yakovleva, A. V. Sivtseva |
| DOI | 10.17073/1997-308x.2025.580p.1076 |
Thermal modification at temperatures up to 550 °C left both diamond cores structurally stable. It effectively removed non-diamond sp² carbon from their surface shells. The powders nevertheless remained distinct after matched treatment. Mechanically ground natural nanodiamond contained 74% plate-shaped particles with 14 to 26 nm in-plane dimensions and 1.5 to 10 nm thickness. Detonation nanodiamond contained 84% isometric particles with 4 to 6 nm crystallites.
Synthesis route sets particle shape and core size
Section titled “Synthesis route sets particle shape and core size”The paper calls mechanically ground natural nanodiamond NND and detonation nanodiamond DND. Natural nanodiamond began as industrial diamond micropowder passed through a 40 μm wire sieve. Repeated direct grinding used a vibrating mill with a tungsten carbide lined steel container. Steel balls measured 6 to 11 mm, and their mass was five times the diamond charge. Wet grinding used ethanol or distilled water to remove heat.
The authors suggest that mechanical loading cleaves the crystals mainly along planes parallel to octahedral faces. They identify these planes as {111}. The authors also associate DND’s isometric shape with its formation during detonation.
Chemical cleaning used sequential boiling mixtures of HNO₃ with H₂SO₄ and HNO₃ with HCl. The powders then received NaOH treatment and repeated distilled-water washing. The dry NND yield was 78 to 85% of the starting diamond mass.
The detonation comparison used UDA-S-GO powder, which had already received deep chemical purification. The comparison therefore represents one mechanically prepared natural powder and one named detonation grade.
Matched annealing and measurement workflow
Section titled “Matched annealing and measurement workflow”Both powders were annealed dry in separate corundum ceramic dishes. The muffle furnace operated in air at atmospheric pressure. Fixed stages were 200, 300, 400, 500, and 550 °C. Samples were removed after 1 hour at each stage, so cumulative exposure rose from 1 to 5 hours.
The authors describe selective oxidation as removal of less stable non-diamond carbon through conversion to CO and CO₂. The nine-method study combined XRD, electron microscopy, Raman spectroscopy, atomic force microscopy, dynamic light scattering, XPS, solid-state NMR, IR spectroscopy, and BET analysis.
Pycnometry measured density, while small-angle X-ray scattering and DLS assessed particle size. XRD used monochromatic Cu Kα radiation with λ = 1.541 Å over 2θ = 17° to 96°. High-resolution TEM used a Titan 80-300 microscope with about 0.08 nm resolution. FFT analysis of lattice fringes supplied particle-level interplanar distances. The paper reserves detailed Raman, IR, XPS, and NMR surface-chemistry analysis for Part 2.
Morphology and bulk physical properties
Section titled “Morphology and bulk physical properties”NND had denser, larger particles with far less surface area. Table 1 summarizes the initial physical properties after chemical cleaning.
Table 1. Initial properties of the natural and detonation nanodiamond powders
| Property | NND | DND |
|---|---|---|
| Particle shape | 74% plate, 19% intermediate, 7% isometric | 84% isometric, 16% intermediate |
| Mean particle size by electron microscopy | 24.0 nm | 5.6 nm |
| Pycnometric density | 3.05 g/cm³ | 2.95 g/cm³ |
| BET specific surface area | 33.4 ± 2.0 m²/g | 338.6 ± 20.3 m²/g |
| Noncombustible residue | 0.95% | 1.1% |
The X-ray estimate described coherent crystallite regions, which differed from whole-particle dimensions. Both pycnometric densities were below the theoretical diamond density of 3.5154 g/cm³. They also fell below the reported 3.30 to 3.60 g/cm³ range for bulk natural crystals.
The authors interpret the high density and low surface area of NND as evidence of larger, denser, smoother particles. Detonation properties are strongly influenced by its shell.
Before annealing, DND formed micron-scale or larger agglomerates in water and other liquids. These agglomerates settled rapidly and prevented DLS from resolving primary particles reliably. After air annealing, DLS in water gave maximum sizes of 28.35 nm for NND and no more than 4.31 nm for DND. The authors interpreted the narrower distributions as lower agglomeration and improved sedimentation stability.
Core lattice and defect density
Section titled “Core lattice and defect density”Nanodiamond cores were cubic in both powders, with diffraction from the (111), (220), and (311) planes. Initial d111 values were 2.067 Å for NND and 2.068 Å for DND. After annealing at 550 °C, they were 2.065 Å and 2.072 Å, respectively.
The (111) coherent scattering domains measured 14.08 nm for NND and 4.16 nm for DND. After annealing, they were 14.23 nm and 4.40 nm. NND had a more perfect lattice and a lower measured defect density.
The average physical broadening of DND diffraction lines was 3.9 times that of NND before and after annealing. High-resolution TEM gave d111 = 2.062 Å for NND and 2.071 Å for DND. The paper uses 2.060 Å for ideal diamond and 1.25 Å for bulk d220. Thus, both nanodiamond lattices exceeded bulk values, but NND stayed closer to the reference.
The increase agrees with prior studies cited by the authors, which link smaller crystallites with larger lattice parameters. NND also produced a better diffraction signal-to-noise ratio.
Preliminary TEM analysis of 12 images found DND dislocation density about twice that of NND. The authors state that a more representative image set is needed for a statistically reliable estimate.
Air annealing cleans the shell without changing the core
Section titled “Air annealing cleans the shell without changing the core”Thermal modification through 550 °C did not measurably alter particle shape or core crystallography. The final 550 °C condition included 5 hours of cumulative exposure. Peak intensity ratios remained about 100:51:18 for NND and 100:21:12 for DND.
The broad diffuse band in initial DND from 2θ = 18° to 28° almost disappeared after annealing. The authors assign this band to amorphous non-diamond carbon. Disappearance indicates removal of that phase or a decrease below XRD detection.
Coherent scattering domain sizes changed little, and the plate and isometric morphologies remained. The reported outcome is selective shell cleaning, with no significant change in the diamond cores. Part 2 will use Raman, IR, XPS, and NMR to examine the shell’s chemical state in detail.
Measurement limits and unresolved questions
Section titled “Measurement limits and unresolved questions”Each size method has a limitation that affects interpretation. Small-angle X-ray scattering loses accuracy for very small and polydisperse particles. It also responds to agglomeration, so its result can represent an aggregate rather than a primary particle. The Scherrer calculation is less reliable for polydisperse crystallites. Dynamic light scattering measures suspended agglomerates and requires a stable dispersion. High-resolution TEM measures individual crystallites but samples few particles.
The combined methods provide mutual verification, which was the reason for using all nine. The authors also note that detonation powder can vary between batches. Synthesis, purification, and surface modification affect its metastable structure. Measured properties should therefore be tied to the specific grade and processing history.
The proposed effects on hydrophilicity, hydrophobicity, conductivity, and colloidal stability remain future targets. Part 1 does not test those functions.
Implications for powder selection
Section titled “Implications for powder selection”Natural nanodiamond offers a larger, denser core with a more perfect lattice and much smaller specific surface area. It may suit applications that prioritize core crystallinity over high surface area. The paper did not test device performance for either powder.
Detonation nanodiamond offers smaller isometric crystallites and about ten times the surface area. Its shell composition and aggregation state remain central to dispersion behavior. Air annealing through 550 °C can reduce non-diamond shell carbon while preserving measured core structure.
For powder selection, compare shape, surface area, lattice deviation, and suspension size under the intended liquid conditions. Do not treat a DLS maximum as an individual crystallite size when agglomeration remains. For these powders, the synthesis route set core morphology and defect density, while the 550 °C air treatment removed shell carbon without changing the measured core.
View Original Abstract
The work presents a comprehensive comparative study of diamond nanoparticles obtained by two fundamentally different methods - mechanical grinding of natural diamond (NND) and detonation synthesis (DND) - in their initial state and after thermal modification in air. The use of a combination of complementary high-resolution analysis methods allowed for the acquisition of reliable and reproducible data on the morphology and crystal structure of both the diamond core and the surface shell of the nanoparticles. The study revealed differences in the structure and morphology of the primary NND and DND particles. NND particles are characterized by a predominantly plate-like morphology (in-plane dimensions 14-26 nm, thickness 1.5-10 nm), a higher pycnometric density, and a lower specific surface area compared to isometric DND particles with a crystallite size of 4-6 nm. It was found that the crystal lattice of the NND core is characterized by a higher degree of perfection and a lower density of defects, which is confirmed by X -ray diffraction and high-resolution transmission electron microscopy data, as well as by smaller deviations of the interplanar distances from the values characteristic of bulk diamond. An increase in interplanar distances with decreasing crystallite size was observed: the mean interplanar distances, and therefore the lattice parameters of DND nanocrystals, are significantly larger than those of NND nanocrystals. In turn, the lattice parameters of NND slightly exceed those of bulk diamond, which experimentally confirms previous findings that the lattice parameter increases as the size of nanodiamond crystallites decreases. Thermal modification at temperatures up to 550 °C does not significantly affect the morphology and crystal structure of the diamond core of either NND or DND, while ensuring effective removal of non-diamond sp² carbon from their surface shell.
Advanced Thermal Simulation Service Diamond Heat Spreader Performance Analysis
View Specs →
Electronic Grade Intrinsic Diamond Epitaxial Wafer H Terminated Superior 100 Mosfet Ready Substrate