Direct observation of electron emission from grain boundaries in CVD diamond by PeakForce-controlled tunnelling atomic force microscopy
At a Glance
Section titled “At a Glance”| Metadata | Details |
|---|---|
| Publication Date | 2015-07-04 |
| Journal | Carbon |
| Authors | Robert L. Harniman, Oliver Fox, Wiebke Janssen, Sien Drijkoningen, Ken Haenen |
| Institutions | University of Bristol, Hasselt University |
| Citations | 65 |
| Analysis | Full AI Review Included |
Direct Observation of Electron Emission from Grain Boundaries in CVD Diamond via PF-TUNA
Section titled “Direct Observation of Electron Emission from Grain Boundaries in CVD Diamond via PF-TUNA”Executive Summary
Section titled “Executive Summary”- Objective: Direct visualization and quantification of electron field emission sites on polycrystalline CVD diamond films using PeakForce-controlled tunnelling atomic force microscopy (PF-TUNA).
- Key Finding: Electron emission originates preferentially from grain boundaries, not from topographical peaks or sharp edges, effectively debunking the need for geometric field enhancement in diamond cold cathodes.
- Grain Size Correlation: Emission area scales inversely with grain size: Undoped MCD (18%) → NCD (26%) → UNCD (49%).
- Doping Effects: Light N, B, or P doping broadens emission sites along grain boundaries; heavy B-doping (~9 × 1020 cm-3) results in near-metallic conductivity with uniform emission across both grains and boundaries (80-90% surface area).
- Phosphorus Anomaly: Light P-doping induces micro-stepped (111) facets that act as dense emission networks, surpassing even UNCD with 62% emitting surface area.
- Temporal Instability: Measured emission current decays to ~10% of its initial value within 30 hours of ambient exposure, attributed to surface adsorbates and transfer doping.
- Engineering Implication: Flat, heavily doped, or nanocrystalline diamond wafers provide superior field emission without complex microfabrication of conical or needle-like structures.
Technical Specifications
Section titled “Technical Specifications”| Parameter | Value | Unit | Context |
|---|---|---|---|
| Film Thickness (MCD/NCD) | ~5 | µm | Undoped & N-doped films |
| Film Thickness (P-doped) | ~2.5 | µm | Phosphorus-doped MCD |
| Film Thickness (Heavy B-doped) | ~3 | µm | High boron concentration |
| Substrate Resistivity (P-doped) | 10-20 | kΩ·cm | Highly resistive Si (100) |
| Deposition Pressure (N-doped) | 110 | Torr | MWCVD reactor |
| Deposition Pressure (P-doped) | 50 | Torr | ASTeX PDA-18 reactor |
| Substrate Temperature (P-doped) | 820 | °C | P-doped MCD growth |
| Microwave Power (N-doped) | 1.0 | kW | NCD deposition |
| Microwave Power (P-doped) | 5.0 | kW | MWCVD reactor |
| Methane Concentration (N-doped) | 6.5% | CH4/H2 | Renucleation conditions |
| Methane Concentration (P-doped) | 1% | CH4/H2 | Microcrystalline growth |
| Light B-doping (B2H6) | ~50 | ppm | B concentration ~2.4 × 1019 cm-3 |
| Heavy B-doping (B2H6) | ~10,000 | ppm | B concentration ~9 × 1020 cm-3 |
| P-doping (PH3) | 10,000 | ppm P/C | Estimated P ~1 × 1019 cm-3 |
| Resistivity (Undoped MCD/NCD) | >10 | MΩ | Highly insulating |
| Resistivity (Light B-doped) | ~160 | kΩ | p-type semiconductor |
| Resistivity (Heavy B-doped) | ~100 | Ω | Near-metallic |
| Activation Energy (N in diamond) | 1.7 | eV | High; causes passivation |
| AFM Cantilever Spring Constant | 0.4 | N/m | PtIr-coated tip |
| Tip Radius | 20 | nm | Nominal PtIr coating |
| Tip-Sample Bias | 1 mV - 1 V | — | Tunnelling regime |
| Tip-Sample Gap | ~1 | nm | PeakForce controlled |
| Emission Current Range | pA - hundreds of pA | — | Per emission site |
| Bake Temperature | 200 | °C | Vacuum recovery test |
| Emission Decay Time | ~30 | hours | ~90% reduction post-exposure |
Key Methodologies
Section titled “Key Methodologies”- Substrate Preparation: Diamond deposition on highly resistive Si (100) substrates (10-20 kΩ·cm) to enable back-contact biasing.
- MPCVD/MWCVD Growth:
- Undoped MCD: Standard CH4/H2 chemistry, H-terminated.
- UNCD: Inert gas addition (Ar) for renucleation, grain size <10 nm.
- N-doped NCD: 6.5% CH4/0.7% N2/H2 at 110 Torr, 1 kW.
- P-doped MCD: 1% CH4/H2 + PH3 at 50 Torr, 820°C.
- Light B-doped: +50 ppm diborane.
- Heavy B-doped: +10,000 ppm diborane.
- Hydrogen Termination: Post-deposition H-plasma exposure to establish surface conductivity.
- Electrical Contacting: Conductive silver paint attaching Si substrate to steel disc; bias applied between grounded sample and AFM tip.
- PF-TUNA Imaging: Multi-mode VIII AFM with PF-TUNA module, PeakForce feedback, PtIr cantilevers (k = 0.4 N/m), 5120 × 5120 pixel resolution, 0.1 Hz scan rate.
- Threshold Analysis: Quantification of emitting surface area via RMS current threshold; comparison across samples using relative percentage methodology.
- Aging Studies: Ambient exposure monitoring with 200°C vacuum bake recovery tests.
6CCVD Solutions & Capabilities
Section titled “6CCVD Solutions & Capabilities”The findings in this paper — particularly the dominance of grain boundary emission and the exceptional performance of nanocrystalline and heavily boron-doped morphologies — align directly with 6CCVD’s manufacturing portfolio for vacuum electronic and cold cathode applications.
Applicable Materials
Section titled “Applicable Materials”- Optical Grade PCD & Heavy Boron-Doped PCD (BDD): The heavy B-doped MCD films (~9 × 1020 cm-3) producing 80-90% uniform emission correspond to 6CCVD’s Heavy Boron-Doped PCD line, where near-metallic resistivity enables uniform electron emission without microfabricated emitter tips.
- Nanocrystalline Diamond (NCD/UNCD): The inverse grain-size/emission relationship validates 6CCVD’s NCD/UNCD PCD wafers for flat-panel cold cathode arrays, eliminating the need for complex tip-sharpening lithography.
- Intrinsic & Lightly Doped PCD: For controlled grain boundary emission studies, 6CCVD supplies Optical Grade PCD with custom grain size distributions grown via MPCVD.
Customization Potential
Section titled “Customization Potential”- Doping Precision: 6CCVD’s MPCVD reactors enable calibrated B, N, and P doping across the full spectrum used in this work — from insulating (>10 MΩ) to near-metallic (~100 Ω) regimes.
- Wafer Dimensions: While this study used small Si-supported films, 6CCVD manufactures freestanding PCD plates up to 125mm in diameter, enabling large-area field emitter arrays for commercial flat-panel displays and accelerator RF injectors.
- Thickness Control: Films can be supplied from 0.1 µm to 500 µm (PCD/SCD) and up to 10mm for substrates — critical for managing back-contact resistance and mechanical robustness in vacuum devices.
- Surface Engineering: 6CCVD offers polishing to Ra < 5nm on inch-size PCD, addressing the temporal instability issue highlighted in this paper by providing smooth, controlled surfaces for reproducible emission characterization.
- Metalization: For device integration, 6CCVD provides in-house metalization (Ti, Pt, Au, W, Cu, Pd) to facilitate back-contacts and electrode patterning required for field emitter array fabrication.
- Laser Cutting: Custom geometries (including the high-density emitter arrays implied by this research) can be achieved through 6CCVD’s laser cutting services.
Engineering Support
Section titled “Engineering Support”6CCVD’s in-house PhD engineering team can assist with:
- Selecting the optimal grain size-to-doping ratio for specific field emission targets.
- Replicating the micro-stepped (111) P-doped morphology observed in this study for enhanced step-edge emission sites.
- Designing H-terminated surface protocols to maximize the initial emission current and minimize the ~90% ambient decay documented in the aging studies.
- Advising on vacuum storage and transfer best practices to preserve surface transfer doping effects.
Call to Action
Section titled “Call to Action”For custom specifications, tailored doping concentrations, or material consultation on diamond cold cathode and field emitter projects, visit 6ccvd.com or contact our engineering team directly.
View Original Abstract
A detailed investigation of electron emission from a set of chemical vapour deposited (CVD) diamond films is reported using high-resolution PeakForce-controlled tunnelling atomic force microscopy (PF-TUNA). Electron field emission originates preferentially from the grain boundaries in low-conductivity polycrystalline diamond samples, and not from the top of features or sharp edges. Samples with smaller grains and more grain boundaries, such as nanocrystalline diamond, produce a higher emission current over a more uniform area than diamond samples with larger grain size. Light doping with N, B or P increases the grain conductivity, with the result that the emitting grain-boundary sites become broader as the emission begins to creep up the grain sidewalls. For heavy B doping, where the grains are now more conducting than the grain boundaries, emission comes from both the grain boundaries and the grains almost equally. Lightly P-doped diamond samples show emission from step-edges on the (1 1 1) surfaces. Emission intensity was time dependent, with the measured current dropping to ∼10% of its initial value ∼30 h after removal from the CVD chamber. This decrease is ascribed to the build-up of adsorbates on the surface along with an increase in the surface conductivity due to surface transfer doping.
Tech Support
Section titled “Tech Support”Original Source
Section titled “Original Source”References
Section titled “References”- 2008 - Forms and behaviour of vacuum emission electronic devices comprising diamond or other carbon cold cathode emitters [Crossref]
- 2011 - A review of recent results on diamond vacuum lateral field emission device operation in radiation environments [Crossref]
- 2014 - Planar ultrananocrystalline diamond field emitter in accelerator radio frequency electron injector: Performance metrics [Crossref]
- 2014 - High quantum efficiency ultrananocrystalline diamond photocathode for photoinjector applications [Crossref]
- 2012 - Field emission from diamond-coated multiwalled carbon nanotube ‘teepee’ structures [Crossref]
- 2013 - An increase in the field emission from vertically aligned multiwalled carbon nanotubes caused by NH3 plasma treatment [Crossref]
- 2002 - Can we reliably estimate the emission field and field enhancement factor of carbon nanotube film field emitters? [Crossref]
- 2001 - Field emission from short and stubby vertically aligned carbon nanotubes [Crossref]
- 2008 - Highly resilient field emission from aligned single-walled carbon nanotube arrays chemically attached to n-type silicon [Crossref]
- 1998 - A new surface electron-emission mechanism in diamond cathodes [Crossref]