Down-scaling grating couplers and waveguides in single-crystal diamond for VIS-UV operation
At a Glance
Section titled “At a Glance”| Metadata | Details |
|---|---|
| Publication Date | 2018-12-07 |
| Journal | Journal of Physics Photonics |
| Authors | Fei Gao, Jürgen Van Erps, Zhihong Huang, Hugo Thienpont, Raymond G. Beausoleil |
| Institutions | Vrije Universiteit Brussel, Hewlett-Packard (United States) |
| Citations | 5 |
| Analysis | Full AI Review Included |
Executive Summary
Section titled “Executive Summary”- First-ever VIS-UV grating couplers and waveguides on SCD thin films, experimentally demonstrating operation at 850 nm, 635 nm, and 405 nm wavelengths for photonic integrated circuits.
- Novel tilted-etching (RIE) technique reduces diamond substrate wedge by 60%, from 300 to 120 nm mm-1, enabling uniform thin-film processing critical for short-wavelength nanophotonic fabrication.
- High-performance photonic devices fabricated on Type II(a) SCD using electron-beam lithography (EBL) and reactive-ion etching (Ar/O2 plasma), achieving grating periods down to 254 nm.
- Measured optical losses: 20.6 dB / 22.7 dB total grating coupling loss at 850 nm / 635 nm; waveguide propagation losses of 11 dB mm-1 and 20.5 dB mm-1, respectively.
- 405 nm operation confirmed with 33.1 dB coupling loss and 46.7 dB mm-1 waveguide loss, extending SCD photonic capability into the UV domain.
- Pivotal for quantum photonics, enabling efficient fiber-to-chip coupling for NV− and SiV− color centers, and supporting on-chip VIS supercontinuum generation and wavelength conversion.
- CMOS-compatible and wafer-scale approach replaces traditional microscope objective or fiber-taper coupling, enabling automated testing and scalable photonic networks.
Technical Specifications
Section titled “Technical Specifications”| Parameter | Value | Unit | Context |
|---|---|---|---|
| Target Operating Wavelengths | 850, 635, 405 | nm | VIS-UV short-wavelength operation |
| Grating Periods | 560, 401, 254 | nm | For 850/635/405 nm devices |
| Grating Fill Factors | 0.41, 0.43, 0.41 | - | TE-polarized transmission optimization |
| SCD Thin Film Thickness | ~250 | nm | Target for 850/635 nm devices |
| SCD Material Type | Type II(a) | - | Electronic grade, low nitrogen |
| Refractive Index (SCD @ 635 nm) | 2.412 | - | High index for tight confinement |
| Raman Gain (@ 1030 nm) | 13.5 ± 2.0 | cm GW-1 | On-chip wavelength conversion |
| Kerr Nonlinearity (NIR) | 8.2 ± 3.5 × 10-20 | m2 W-1 | Frequency comb generation |
| Raman Shift | 40 | THz | Exceptionally large |
| Initial Wafer Wedge | 300 | nm mm-1 | From commercial SCD plates |
| Reduced Wafer Wedge (tilted-etch) | 120 | nm mm-1 | 60% reduction achieved |
| Diamond Etch Rate (Ar/Cl2) | 39.1 | nm min-1 | Tilted-etching condition |
| Wedge Reduction Rate | 2.02 | nm mm-1 min-1 | Tilted-etching performance |
| Etch Mask | XR1541 e-beam resist, 100 nm thick | - | Spin-coated |
| SiO2 Cladding Thickness | 2 µm | - | Top and bottom cladding |
| Total Grating Coupling Loss | 20.6 (850 nm), 22.7 (635 nm), 33.1 (405 nm) | dB | Input + output combined |
| Waveguide Propagation Loss | 11, 20.5, 46.7 | dB mm-1 | At 850/635/405 nm |
| -3 dB Bandwidth | 52, 26, 17 | nm | At 850/635/405 nm |
| Peak Transmission Wavelengths | 863, 632, 411 | nm | Measured values |
| Waveguide Length (max) | 370 | µm | Fabricated devices |
| Surface Roughness (Rq) | ~4 | nm | AFM measurement on taper region |
| Tilt Angle During Etching | ~45 | ° | Mounted on metal holder |
| SCD Plate Starting Thickness | 5 | µm | Mechanical polished plate |
| Plasma Chemistry | Ar/Cl2 (thinning), Ar/O2 (RIE) | - | Dry-etching processes |
Key Methodologies
Section titled “Key Methodologies”- Substrate Preparation: Start with 3 × 3 mm2, 5 µm thick synthetic SCD plates (MBOptics); fragment into 1 mm2 shards and transfer onto Si carriers with 2 µm thermal SiO2.
- Tilted-Etching for Wedge Reduction: Mount carrier wafer at ~45° tilt angle in RIE chamber; use Ar/Cl2 plasma to create electric-field gradient, achieving higher etch rate on thicker side of diamond.
- Multi-Step Thinning: Reduce diamond thickness to ~1 µm, transfer to fresh carrier, resume thinning to target 250 nm. Etch rate of 39.1 nm min-1 at 30 min intervals.
- EBL Patterning: Spin-coat 100 nm of Dow Corning XR1541 e-beam resist (6% concentration); expose patterns using Raith 150-two EBL tool.
- Development: Use AZ300 MIF developer to reveal grating and waveguide patterns.
- Reactive-Ion Etching: Transfer patterns into diamond film using Ar/O2 plasma chemistry for grating definition.
- Resist Stripping: Remove residual e-beam resist using secondary Ar/Cl2 plasma step.
- Cladding Deposition: Grow 2 µm SiO2 top cladding via plasma-enhanced chemical vapor deposition (PECVD) to reduce scattering losses.
- Optical Characterization: Use 842 nm (Thorlabs LP852-SF30), 635 nm (Thorlabs S1FC635), and 405 nm (Coherent) CW lasers with tapered (50 µm core) and lensed (9 µm core) fibers for transmission measurements.
6CCVD Solutions & Capabilities
Section titled “6CCVD Solutions & Capabilities”Applicable Materials
Section titled “Applicable Materials”| 6CCVD Product | Application Match |
|---|---|
| Optical Grade Single Crystal Diamond (SCD) | Directly applicable for VIS-UV grating couplers and waveguide fabrication; required Type II(a) electronic-grade material with low nitrogen for minimal absorption across 405-850 nm range. |
| Ultra-Thin SCD Membranes (down to 0.1 µm) | Matches the 250 nm thin-film requirement; 6CCVD provides custom thinning services to achieve sub-micron uniform membranes. |
| MPCVD-Grown SCD Films | Superior alternative to mechanical-polished plates; eliminates wedge issues at source by providing as-grown uniform thickness profiles, bypassing the need for post-process tilted-etching compensation. |
Customization Potential
Section titled “Customization Potential”- Ultra-Low Wedge Wafers: 6CCVD can deliver SCD plates with minimized wedge (< 50 nm mm-1) through precision MPCVD growth and advanced polishing protocols, eliminating the need for complex tilted-etching compensation.
- Custom Thickness Control: Films from 0.1 µm to 500 µm available for SCD; substrates up to 10 mm for thick device platforms.
- Wafer Dimensions: Plates up to 125 mm diameter for scalable, wafer-scale photonic integration—ideal for transitioning this research to commercial production.
- Surface Roughness Optimization: 6CCVD offers Ra < 1 nm polishing for SCD surfaces, directly reducing sidewall scattering losses that currently limit waveguide propagation efficiency at short wavelengths.
- Laser Cutting Services: Custom shaping and dicing of SCD plates to specific shard dimensions (e.g., 1 mm2 or 3 × 3 mm2) for device fabrication workflows.
Engineering Support
Section titled “Engineering Support”6CCVD’s in-house PhD engineering team specializes in SCD material selection for advanced photonic integrated circuits, quantum photonics (NV−/SiV− center applications), and nonlinear optics. Our team can assist with:
- Material specification for short-wavelength VIS-UV photonic devices
- Custom geometry design for waveguide and resonator fabrication
- Thickness optimization to minimize propagation losses
- Substrate selection guidance for quantum emitter integration
Call to Action: For custom specifications, material consultation, or to discuss your VIS-UV diamond photonic project, visit 6ccvd.com or contact our engineering team directly.
View Original Abstract
We report on the design, fabrication and experimental demonstration of single-crystal diamond (SCD) waveguide devices with integrated grating couplers optimized for 850 nm, 635 nm, and 405 nm wavelengths, respectively. The devices are fabricated on SCD thin films using electron-beam lithography and reactive-ion etching technologies. To reduce the wafer wedge typically present in commercial diamond plates, we introduce a novel tilted-etching technique in the preparation of the thin films. We obtain 60% reduction of the wafer wedge, namely from 300 to 120 nm mm -1 , enabling us to properly fabricate the devices designed for the short to ultra-short wavelengths considered here. Using light in- and out-coupling with 50 μ m core tapered fibers, we measure total (input plus output) grating coupling losses of 20.6 dB and 22.7 dB, and waveguide losses of 11 dB mm -1 and 20.5 dB mm -1 for the 850 nm and 635 nm wavelength devices, respectively. The 405 nm wavelength devices, tested with a lensed 9 μ m core input fiber and with the same tapered output fiber as employed for the other devices, also demonstrate light guidance, and feature total grating coupling and waveguide losses on the order of 33.1 dB and 46.7 dB mm -1 , respectively. These results showcase the possibility of down-scaling grating-coupled SCD devices for VIS-UV operation, and pave the way for exploiting diamond’s properties on photonic chips at extremely short wavelengths.