Single-crystalline boron-doped diamond superconducting quantum interference devices with regrowth-induced step edge structure
At a Glance
Section titled “At a Glance”| Metadata | Details |
|---|---|
| Publication Date | 2019-10-23 |
| Journal | Scientific Reports |
| Authors | Taisuke Kageura, Masakuni Hideko, Ikuto Tsuyuzaki, Aoi Morishita, Akihiro Kawano |
| Institutions | Waseda University, National Institute for Materials Science |
| Citations | 14 |
| Analysis | Full AI Review Included |
Executive Summary
Section titled “Executive Summary”- Research achievement: The study reports the first dc-SQUID fabricated from single-crystalline boron-doped diamond, operating above 2 K through a regrowth-induced step-edge Josephson junction.
- Device architecture: A superconducting-weak-superconductor-superconducting (S-S′-S) junction was formed using an undoped diamond regrowth layer and a crystallographically controlled step.
- Critical process parameter: The step angle, controlled by the ratio of undoped-layer thickness to etched-step height and by CO2 addition, directly determines junction formation and weak-link behavior.
- Electrical performance: The junction achieved a critical current density of 5800 A/cm2 at 1.6 K, with non-hysteretic current-voltage characteristics.
- SQUID performance: The device demonstrated periodic flux-voltage modulation at 2.6 K, with an average peak-to-peak modulation of approximately 0.8 µV and a field period of 0.43 µT.
- Material advantage: Single-crystalline boron-doped diamond provides a potentially higher operating temperature, high critical field, mechanical robustness, oxidation resistance, and compatibility with epitaxial diamond processing.
- Engineering significance: The process offers a route toward higher-temperature diamond SQUIDs, simpler 4He cryogenics, scanning magnetic microscopy, and hybrid quantum systems incorporating nitrogen-vacancy centers.
Technical Specifications
Section titled “Technical Specifications”| Parameter | Value | Unit | Context |
|---|---|---|---|
| Substrate orientation | (111) | — | HPHT single-crystalline diamond substrate |
| Step height, h | 230-400 | nm | Oxygen-plasma-etched vertical step |
| Undoped regrowth-layer thickness, dUN | 0-300 | nm | Homoepitaxial MPCVD layer |
| Investigated step angles | 85, 80, 50, 20 | ° | Step angle between substrate surface and step |
| Step-angle control ratio, dUN/h | 0, 0.5, 1.0 | — | Lateral-growth conditions |
| Selected SQUID step height | 230 | nm | Fabricated dc-SQUID |
| Selected SQUID undoped-layer thickness | 230 | nm | Fabricated dc-SQUID |
| Selected SQUID boron-doped-layer thickness | 180 | nm | Selective epitaxial superconducting layer |
| Selected SQUID step angle | 50 | ° | Weak-link-forming condition |
| Boron-doping threshold for superconductivity | Greater than 3 × 1020 | cm−3 | Approximate threshold reported in the paper |
| Highest reported TC for (111) single-crystalline diamond | 10 | K | Literature value cited by the authors |
| Upper critical magnetic field | Above 10 | T | Literature value for high-quality superconducting diamond |
| Regrowth methane concentration, standard condition | 0.05 | % | CH4 diluted in hydrogen |
| Regrowth total gas flow | 400 | sccm | Standard step-angle conditions |
| Regrowth pressure | 35 | Torr | Standard step-angle conditions |
| Regrowth substrate temperature | 620 | °C | Standard step-angle conditions |
| Standard regrowth growth rate | 41.7 | nm/h | Estimated using secondary-ion mass spectrometry |
| CO2-assisted methane concentration | 0.75 | % | Condition used to produce the 20° step |
| CO2 concentration | Not specified in extracted text | — | Added during regrowth for step-angle reduction |
| Oxygen-etch gas flow | 45 | sccm | ICP-RIE step formation |
| Oxygen-etch pressure | 1.4 | Pa | ICP-RIE step formation |
| ICP antenna power | 700 | W | Diamond etching |
| ICP bias power | 100 | W | Diamond etching |
| Diamond etching rate | 220 | nm/min | Stylus-profilometer measurement |
| Ti/Au contact thickness | 30/100 | nm | Titanium adhesion layer and gold contact |
| Contact anneal temperature | 500 | °C | Vacuum anneal |
| Contact anneal vacuum | Greater than 1 × 10−5 | Pa | Improves Ti/diamond adhesion |
| Josephson-junction measurement range | 1.6-3.4 | K | Temperature-dependent I-V characterization |
| Junction critical current at 1.6 K | 0.37 | mA | Defined at a 1 µV voltage criterion |
| Junction normal-state resistance | 1.25 | Ω | Estimated from the I-V slope |
| Maximum junction critical current density | 5800 | A/cm2 | At 1.6 K |
| Maximum ICRn | 0.47 | mV | At 1.6 K |
| Estimated junction capacitance | Less than 0.56 | pF | Derived from the non-hysteretic RCSJ analysis |
| Weak-link thickness, dJ | 300 | nm | Estimated for h = 230 nm and α = 50° |
| Coherence length of the weak (001) layer | 7.89 | nm | Literature value at TC = 3.2 K |
| SQUID superconducting-film width | 36 | µm | Fabricated SQUID geometry |
| SQUID loop area | 32 × 32 | µm2 | Geometric loop area |
| Effective SQUID loop area | 68 × 68 | µm2 | Includes the Meissner-effect correction |
| SQUID resistance-transition range | 2-12 | K | Four-probe measurement |
| SQUID first transition: onset/offset | 10.0/9.0 | K | Main superconducting transition |
| SQUID second transition: onset/offset | 4.0/2.8 | K | Step-region weak superconducting transition |
| SQUID non-hysteretic I-V range | 2.2-4.0 | K | Reported operating range |
| SQUID operation temperature | 2.6 | K | Flux-voltage modulation demonstrated |
| Measured SQUID field period | 0.43 | µT | Periodic voltage modulation |
| Theoretical field period | 0.45 | µT | Calculated from Φ0/Aeff |
| Average voltage modulation | Approximately 0.8 | µV | Peak-to-peak value |
| Flux quantum, Φ0 | 2.07 × 10−15 | Wb | Used in the RCSJ and SQUID calculations |
| Microwave frequency used for Shapiro response | 10 | GHz | Measurement condition |
| Microwave power | 11.2 | dBm | Measurement condition |
| Measured Shapiro step | Approximately 20 | µV | Close to the theoretical 20.7 µV step |
| TEM accelerating voltage | 200 | kV | Cross-sectional structural analysis |
| Measurement systems | PPMS and MPMS | — | Quantum Design systems used for transport and magnetic measurements |
| Measurement configuration | Four-probe | — | Electrical resistance characterization |
Key Methodologies
Section titled “Key Methodologies”-
Prepare the single-crystalline substrate
- Use a commercially available HPHT single-crystalline diamond substrate with a (111) orientation.
- Clean the surface using a boiled acid mixture of HNO3 and H2SO4 at a 1:3 ratio.
- Perform the treatment at 200 °C for 30 min.
- Rinse with deionized water and terminate the surface with oxygen using UV exposure in oxygen for 3 h at room temperature.
-
Form the initial nickel etch mask
- Define the step pattern by photolithography.
- Deposit nickel by electron-beam evaporation.
- Remove the resist and complete the selective nickel-mask pattern by lift-off.
-
Etch the diamond step
- Perform O2 inductively coupled plasma reactive-ion etching.
- Use 45 sccm O2, 1.4 Pa pressure, 700 W antenna power, and 100 W bias power.
- Use the reported etching rate of 220 nm/min to obtain step heights of 230-400 nm.
- Remove the nickel mask using acid treatment.
-
Grow the undoped diamond regrowth layer
- For the 85°, 80°, and 50° steps, use:
- CH4 concentration: 0.05% in hydrogen.
- Total flow: 400 sccm.
- Pressure: 35 Torr.
- Substrate temperature: 620 °C.
- Vary the undoped-layer thickness to control dUN/h and thereby adjust the step angle.
- The standard growth rate was approximately 41.7 nm/h.
- For the 85°, 80°, and 50° steps, use:
-
Produce the 20° step condition
- Add CO2 during regrowth.
- Increase the methane concentration to 0.75% in hydrogen.
- Retain the total flow at 400 sccm.
- The extracted text does not specify the CO2 flow or concentration.
-
Define the junction and SQUID pattern
- Form a Ti/Au stacked mask by photolithography, electron-beam evaporation, and lift-off.
- Use 30 nm Ti and 100 nm Au.
-
Grow the superconducting boron-doped layer
- Selectively epitaxially grow the boron-doped diamond layer by MPCVD.
- Use identical superconducting-growth conditions for all samples.
- Control layer thickness through growth time.
- The SQUID device used a boron-doped layer thickness of 180 nm.
-
Remove the metal mask
- Remove the Ti/Au mask by acid treatment after selective epitaxial growth.
- Deposit four Ti/Au contact pads for four-probe transport measurements.
- Anneal the contacts at 500 °C under vacuum better than 1 × 10−5 Pa.
-
Characterize the structure
- Examine step morphology using high-resolution FE-SEM.
- Analyze cross-sectional crystallography using TEM at 200 kV.
- Prepare TEM lamellae using a focused-ion-beam system.
- Determine step orientation using X-ray diffraction pole-figure measurements.
-
Measure electrical transport
- Measure resistance using the four-probe method.
- Define IC as the current required to reach 1 µV.
- Calculate critical current density using IC/S, where S is the superconducting-film cross-sectional area.
- Measure I-V behavior, temperature-dependent resistance, Shapiro steps, and SQUID flux-voltage modulation.
- Bias the SQUID above its critical current and apply a perpendicular magnetic field.
6CCVD Solutions & Capabilities
Section titled “6CCVD Solutions & Capabilities”Applicable Materials
Section titled “Applicable Materials”| 6CCVD material or structure | Suitability for this research | Recommended use |
|---|---|---|
| Single-crystal diamond, SCD, (111)-oriented | Required to reproduce the epitaxial regrowth and orientation-dependent weak-link structure | Substrate and homoepitaxial device platform |
| Optical Grade SCD | Suitable when low surface roughness, crystallographic quality, and device-grade surfaces are required | Polished substrates for lithography, selective growth, and Josephson-device fabrication |
| Boron-doped SCD | Primary conductive and superconducting material; boron concentration must exceed the reported superconducting threshold of approximately 3 × 1020 cm−3 | Superconducting electrodes, weak links, and SQUID structures |
| Heavy boron-doped PCD | Potentially useful for higher-current or larger-area device platforms, although grain boundaries may alter junction behavior | Prototype SQUIDs, magnetic shields, current-carrying layers, and larger superconducting circuits |
| Undoped or low-boron SCD regrowth layer | Essential for producing the S-S′-S weak-link region | Controlled step-edge regrowth between superconducting regions |
| BDD | Appropriate for boron concentration optimization and conductive diamond studies | Calibration layers, electrical contacts, and exploratory superconducting-device designs |
| Boron-doped diamond on insulating diamond | Closely matches the paper’s insulating-substrate/superconducting-film architecture | Reduced substrate conduction and improved device isolation |
The strongest replication route is a custom (111)-oriented optical-grade SCD substrate, followed by MPCVD growth of an undoped SCD regrowth layer and a heavily boron-doped SCD superconducting layer.
Customization Potential
Section titled “Customization Potential”-
Custom dimensions
- SCD and PCD plates or wafers can be supplied up to 125 mm for PCD.
- SCD and PCD thicknesses are available from 0.1 µm to 500 µm.
- Diamond substrates can be supplied up to 10 mm thick.
- The device geometry can be adapted beyond the paper’s 32 × 32 µm2 loop and 36 µm-wide superconducting tracks.
-
Surface preparation
- SCD polishing can achieve Ra < 1 nm.
- Inch-size PCD surfaces can be polished to Ra < 5 nm.
- These finishes are compatible with photolithography, e-beam patterning, selective growth, and oxygen-plasma processing.
-
Orientation and regrowth control
- (111)-oriented SCD is the preferred starting platform for the reported lateral-growth mechanism.
- Regrowth thickness, step height, methane concentration, pressure, temperature, and optional CO2 addition should be specified as process variables rather than assumed material properties.
- The weak-link behavior is highly sensitive to step angle; the paper identifies 50° as the selected junction geometry.
-
Metalization
- The paper uses Ti/Au = 30/100 nm for contact pads and process masks.
- 6CCVD offers internal metalization using Au, Pt, Pd, Ti, W, and Cu.
- A Ti/Au stack is directly aligned with the reported contact architecture.
- For devices requiring alternative contact resistance, thermal budget, adhesion, or packaging requirements, Pt, Pd, W, or Cu metallization can be evaluated.
-
Laser cutting and device shaping
- Custom cutting and shaping can support device isolation, loop definition, chip separation, and integration with cryogenic or magnetic measurement systems.
- Laser-cut features should be specified together with edge quality, kerf, surface damage, and post-cut polishing requirements.
-
Boron concentration and TC optimization
- A development program should characterize boron concentration, sheet resistance, transition temperature, and transport behavior as a function of film thickness and crystal orientation.
- The paper indicates that the undoped or differently oriented step region can have a lower TC than the main superconducting layer.
- Optimization should therefore target the step-region TC, not only the nominal boron concentration of the superconducting electrodes.
Recommended Development Configuration
Section titled “Recommended Development Configuration”| Device region | Recommended 6CCVD solution | Key specification to define |
|---|---|---|
| Insulating substrate | Optical Grade SCD, (111) orientation | Diameter or length, thickness, Ra, orientation accuracy |
| Etched step | SCD substrate with controlled oxygen-plasma etching | Step height of 230-400 nm, target angle 50° |
| Undoped regrowth | Undoped or very low-boron SCD | dUN, typically 230 nm for the demonstrated device |
| Superconducting electrodes | Heavily boron-doped SCD | Boron concentration, thickness, target TC |
| Contact pads | Ti/Au metalization | 30/100 nm stack, pad layout, anneal compatibility |
| Device isolation and packaging | Custom laser cutting and dimensional processing | Loop dimensions, chip boundaries, edge quality |
| Transport validation | Customer-defined four-probe and cryogenic testing | Measurement temperature, field orientation, current criterion |
Engineering Support
Section titled “Engineering Support”6CCVD’s in-house PhD team can assist with material selection and process definition for:
- Single-crystalline boron-doped diamond Josephson junctions
- Step-edge S-S′-S weak-link structures
- dc-SQUIDs and scanning SQUID platforms
- NV-center and superconducting hybrid quantum systems
- Boron concentration, TC, and critical-current optimization
- MPCVD growth and selective epitaxy development
- Custom SCD and PCD substrates with controlled orientation and surface finish
- Ti/Au and alternative metalization integration
- Cryogenic transport structures and contact-pad layouts
For this application, the recommended first engineering milestone is a controlled material stack comprising (111) optical-grade SCD / undoped SCD regrowth / heavily boron-doped SCD, followed by lithographic step formation and Ti/Au contact processing.
For custom specifications or material consultation, visit 6ccvd.com or contact our engineering team directly.
View Original Abstract
Abstract Superconducting quantum interference devices (SQUIDs) are currently used as magnetic flux detectors with ultra-high sensitivity for various applications such as medical diagnostics and magnetic material microstructure analysis. Single-crystalline superconducting boron-doped diamond is an excellent candidate for fabricating high-performance SQUIDs because of its robustness and high transition temperature, critical current density, and critical field. Here, we propose a fabrication process for a single-crystalline boron-doped diamond Josephson junction with regrowth-induced step edge structure and demonstrate the first operation of a single-crystalline boron-doped diamond SQUID above 2 K. We demonstrate that the step angle is a significant parameter for forming the Josephson junction and that the step angle can be controlled by adjusting the microwave plasma-enhanced chemical vapour deposition conditions of the regrowth layer. The fabricated junction exhibits superconductor-weak superconductor-superconductor-type behaviour without hysteresis and a high critical current density of 5800 A/cm 2 .