An integrated nanophotonic quantum register based on silicon-vacancy spins in diamond
At a Glance
Section titled “At a Glance”| Metadata | Details |
|---|---|
| Publication Date | 2019-10-30 |
| Journal | Physical review. B./Physical review. B |
| Authors | C. T. Nguyen, Denis D. Sukachev, Mihir K. Bhaskar, Bartholomeus Machielse, David Levonian |
| Institutions | Harvard University |
| Citations | 185 |
| Analysis | Full AI Review Included |
Executive Summary
Section titled “Executive Summary”- Quantum Network Node Realized: Demonstration of an integrated 2-qubit register using a Silicon-Vacancy (SiV) color center in diamond coupled to a 13C nuclear spin and a nanophotonic cavity.
- Record Coherence Times: Achieved 100 ms coherence for the 13C nuclear memory and single-shot readout fidelity of 0.97 (aligned field) / 0.92 (misaligned field).
- High-Fidelity Bell States: Generated spin-photon Bell states with fidelity F ≥ 0.89(3) and concurrence C ≥ 0.79(7) (error-corrected), plus electron-nuclear Bell states with F ≥ 0.59(4).
- Cavity QED Performance: Achieved Q > 104, mode volume V < 0.6 [λ/(n=2.4)]3, single-photon Rabi coupling g = 2π × 5.6 GHz, cooperativity C = 38.
- Ultralow-Temperature Operation: Full system operated at ∼60 mK in a dilution refrigerator with 6,1,1 T superconducting vector magnet for strain tuning and Zeeman control.
- Advanced Nanofabrication: Used angled Ion Beam Etching (IBE) instead of Faraday cage RIE, with <65 nm implantation apertures patterned via EBL for deterministic SiV placement.
- Spin-Photon Interface Engineering: Time-bin photonic encoding with δt = 30 ns, 5 ns optical pulses, and 12 ns microwave π-pulses at ΩR > 80 MHz.
Technical Specifications
Section titled “Technical Specifications”| Parameter | Value | Unit | Context |
|---|---|---|---|
| SiV optical transition wavelength | ~737 | nm | Zero-phonon line for spin-cycling transitions f↑↑’, f↓↓‘ |
| Ground-state spin-orbit coupling (λgs) | 46 | GHz | Defines orbital structure |
| Excited-state spin-orbit coupling (λes) | 255 | GHz | Defines excited-state dynamics |
| Optimal ground-state strain (Δgs) | > 100 | GHz | Required for efficient MW driving |
| SiV single-photon Rabi frequency (g) | 2π × 5.6 | GHz | Atom-cavity coupling strength |
| Cavity decay rate (κ) | 2π × 33 | GHz | Linewidth of photonic crystal cavity |
| Atomic decay rate (γ) | 2π × 0.1 | GHz | Bare SiV optical linewidth |
| Cooperativity (C = 4g2/κγ) | 38 | - | Deterministic spin-photon interaction threshold C > 1 |
| Cavity quality factor (Q) | > 104 | - | Measured after IBE fabrication |
| Mode volume (V) | < 0.6 [λ/(n=2.4)]3 | - | For optimal emitter placement |
| Cavity tuning range | > 10 | nm | Via N2 condensation + laser blue-tuning |
| Base temperature | ~60 | mK | Bluefors BF-LD250 dilution refrigerator |
| Magnetic field (Bext) | 0.1 - 0.7 | T | Superconducting (6,1,1) vector magnet |
| SiV spin-qubit frequency (f↑↓) | 2 - 20 | GHz | Tunable via strain and field angle |
| Microwave Rabi frequency (ΩR) | up to 2π × 80 | MHz | Fast gating; 12 ns π-pulses |
| Optimal coherence Rabi frequency | 2π × 10 | MHz | Balances gate speed and heating |
| Spin-echo coherence (T2,SiV2) | 30 | µs | With alumina layer, no DD scaling |
| Spin-echo coherence (T2,SiV1) | up to milliseconds (N=24 pulses) | - | Without alumina, T2(N) ∝ N2/3 |
| 13C coherence time (T2*) | 2.2 | ms | Nuclear Ramsey measurement |
| Single-shot readout fidelity (aligned) | 0.97 | - | Threshold: 13 photons in 30 µs |
| Single-shot readout fidelity (misaligned) | 0.92 | - | Threshold: >1 photon in 13 µs |
| SiV initialization/readout fidelity | 0.85 / 0.84 | - | F↑, F↓ |
| Spin-photon Bell state fidelity (raw) | F ≥ 0.70(3) | - | Post-selected on one photon |
| Spin-photon Bell state fidelity (corrected) | F ≥ 0.89(3) | - | Readout-error corrected |
| Spin-photon concurrence (corrected) | C ≥ 0.79(7) | - | Quantifies entanglement |
| Electron-nuclear Bell state fidelity | F ≥ 0.59(4) | - | Limited by 13C init fidelity (0.9) |
| Microwave rethermalization time (τth) | 70 | µs | Sets heating collapse inter-pulse spacing |
| Noise bath strength (b1) | 5 | kHz | Fast Lorentzian bath |
| Noise bath strength (b2) | 180 | kHz | Slow bulk-related bath |
| Spin-cycling cyclicity threshold | > 50 | photons | Enables high-fidelity single-shot readout |
| Surface spin density (σsurf) | 0.067 | spins/nm2 | Estimated from noise model |
| Bulk spin density | ~0.53 | spins/nm3 | ~3 ppm doping, possibly implantation damage |
| Implantation aperture diameter | < 65 | nm | Defined by EBL on PMMA resist |
| SiV annealing temperature | ~1400 | K | UHV vacuum furnace for SiV formation |
| Coplanar waveguide (CPW) impedance | 50 | Ω | Matched to feed lines; 10 nm Ti / 250 nm Au |
| Fiber collection efficiency | > 90 | % | Tapered fiber, in-situ coupling |
| Overall photon collection efficiency | ~40 | % | Limited by APD quantum efficiency |
| Time-bin separation (δt) | 30 | ns | With 5 ns optical pulses |
| Optical pulse width | 5 | ns | Narrow-band reflection over ~100 MHz |
Key Methodologies
Section titled “Key Methodologies”- Substrate Preparation: Diamond with 1.1% natural 13C abundance, polished to optical-grade surface finish; mounted via indium soldering on gold-plated copper holder.
- Nanophotonic Cavity Fabrication: Pattern HSQ (hydrogen silsesquioxane) hard mask via EBL; angled etch using Ion Beam Etching (IBE) for uniform etch rates across the chip (replacing Faraday-cage RIE).
- SiV Implantation: Spin-coat MMA EL11 / PMMA C4 / Espacer; EBL-defined apertures <65 nm aligned to cavity mode maximum; commercial foundry (Innovion) implants Si ions; UHV anneal at ~1400 K forms SiV centers.
- CPW Integration: Ti (10 nm) / Au (250 nm) liftoff process; CPW width 10 µm; tapered near cavity for enhanced MW field; short termination ensures magnetic field maximum.
- Cryogenic Setup: Bluefors BF-LD250 dilution refrigerator with (6,1,1) T superconducting vector magnet; base temperature ~60 mK; oxygen-free copper braids for thermal anchoring.
- Cavity Tuning: Nitrogen gas condensation red-shifts resonance; 100 µW broadband laser blue-tunes via local heating; tuning range >10 nm stable over months.
- Strain Selection Protocol: Measure Δgs at 4 K via spectroscopy; screen for Δgs > 100 GHz; verify spectral stability and spin-photon interface via f↑↑’ - f↓↓’.
- Cavity QED Characterization: Reflectivity fits extract g, κ, γ, and cooperativity C; detuned (Δ > κ) regime for single-shot readout, near-resonant (Δ ≈ 0) regime for high-contrast Bell-state generation.
- Microwave Control: Coplanar waveguide driven by 40 dB attenuator thermalization chain; Rabi oscillations tuned via power scaling; CPMG-N or XY8-N dynamical decoupling sequences.
- Optical Interrogation: Tapered optical fiber for both excitation and collection (reflection mode); time-bin photonic encoding via cascaded AOM, amplitude-EOM, phase-EOM; δt = 30 ns with 5 ns pulses.
- Noise Spectroscopy: Double Electron-Electron Resonance (DEER) to identify g = 2 bath spins; two-Lorentzian noise model (b, τ) for T2 scaling; coherence optimized at ΩR = 2π × 10 MHz.
- Two-Qubit Gate Construction: Maximally entangling gate Rn↑,n↓φ built from N = 8 π-pulses separated by 2τ = 2 × 2.859 µs; unconditional π/2 nuclear rotations via composite MW sequences.
- Readout Correction: Transfer-matrix formalism accounts for SiV (F ≈ 0.85) and 13C (F ≈ 0.72) readout infidelities; bootstrap statistical analysis for correlation histograms.
6CCVD Solutions & Capabilities
Section titled “6CCVD Solutions & Capabilities”This Harvard-led demonstration establishes a benchmark for integrated quantum photonics using diamond color centers. 6CCVD provides the foundational material building blocks required to replicate or extend this research.
Applicable Materials
Section titled “Applicable Materials”| 6CCVD Product | Relevance to Research |
|---|---|
| Optical Grade SCD (Single Crystal Diamond) | Required substrate for SiV implantation; isotopically engineered 12C options available to suppress nuclear spin bath (paper notes 1% 13C is a major decoherence source). |
| Heavy Boron-Doped PCD | Suitable for superconducting stripline CPW replacements (proposed in the paper to mitigate heating and address all devices simultaneously). |
| Custom-Thickness SCD Wafers | Needed for membrane-style photonic crystal nanobeam fabrication; 6CCVD offers 0.1 µm to 500 µm thickness range with sub-nm Ra polishing. |
| Large-Area PCD Substrates | Up to 125 mm wafers support en-masse fabrication of nanophotonic arrays (paper highlights this as essential for scaling). |
Customization Potential
Section titled “Customization Potential”- Implantation-Ready Surfaces: 6CCVD’s Ra < 1 nm polishing for SCD delivers the optical-grade surface finish required before EBL patterning and ion implantation.
- Custom Metalization: The paper’s CPW uses Ti (10 nm) / Au (250 nm). 6CCVD offers in-house metalization with Au, Pt, Pd, Ti, W, and Cu; thicknesses and geometries are tunable for impedance-matched (50 Ω) coplanar waveguides, with the option for superconducting variants.
- Laser Cutting & Dicing: Diamond chip singulation, cavity-array definition, and undercut etching geometries are supported via 6CCVD’s laser processing capabilities.
- Isotopic Engineering: Consultation available for isotopically purified 12C diamond to extend T2 beyond the 100 ms nuclear coherence benchmark.
- Substrate Geometries: Rectangular membranes, tapered nanobeams, and undercut photonic crystal structures can be sourced as custom orders.
Engineering Support
Section titled “Engineering Support”6CCVD’s in-house PhD team can assist with material selection across the full stack required for cavity-QED quantum networking:
- Substrate Selection: SCD vs. PCD, isotopic purity, crystal orientation (<111> preferred for SiV alignment per paper findings).
- Polishing Specification: Sub-nm Ra surfaces to minimize scattering losses and ensure reproducible cavity Q factors > 104.
- Metalization Stack Design: Adhesion-layer optimization, superconducting CPW transitions, and thickness control to avoid cavity photon absorption (paper notes Q degrades with Au > 300 nm).
- Thermal Management: Material choices for mK-operation dilution-refrigerator mounting, including high-thermal-conductivity diamond geometries.
- Application Consultation: Direct support for quantum network node development, SiV-based quantum memory, cavity QED experiments, and spin-photon entanglement protocols.
Call to Action
Section titled “Call to Action”For custom specifications, isotopic engineering consultation, or material selection for your quantum photonics project, visit 6ccvd.com or contact our engineering team directly.
View Original Abstract
We realize an elementary quantum network node consisting of a silicon-vacancy (SiV) color center inside a diamond nanocavity coupled to a nearby nuclear spin with 100 ms long coherence times. Specifically, we describe experimental techniques and discuss effects of strain, magnetic field, microwave driving, and spin bath on the properties of this 2-qubit register. We then employ these techniques to generate Bell-states between the SiV spin and an incident photon as well as between the SiV spin and a nearby nuclear spin. We also discuss control techniques and parameter regimes for utilizing the SiV-nanocavity system as an integrated quantum network node.