Study of ion-implanted nitrogen related defects in diamond Schottky barrier diode by transient photocapacitance and photoluminescence spectroscopy
At a Glance
Section titled “At a Glance”| Metadata | Details |
|---|---|
| Publication Date | 2021-01-25 |
| Journal | Japanese Journal of Applied Physics |
| Authors | Junjie Guo, Aboulaye Traoré, Masahiko Ogura, Muhammad Hafiz Bin Abu Bakar, Satoshi Yamasaki |
| Institutions | National Institute of Advanced Industrial Science and Technology, Kanazawa University |
| Citations | 4 |
| Analysis | Full AI Review Included |
Executive Summary
Section titled “Executive Summary”- Research Focus: Investigation of electrical control over Nitrogen-Vacancy (NV) center charge states in diamond Schottky barrier diodes using Transient Photocapacitance (TPC) spectroscopy and Photoluminescence (PL) spectroscopy.
- Fabrication Method: Vertical Schottky diodes built on IIb high-pressure/high-temperature (001) diamond substrates, utilizing a 1 µm thick slightly boron-doped homoepitaxial diamond layer grown by Microwave Plasma Chemical Vapor Deposition (MPCVD).
- Defect Engineering: Nitrogen ions implanted at 80 keV (mean depth ~100 nm) with a dose of 1012 ions/cm2 at 600 °C, followed by 1000 °C annealing for 1 hour to form NV centers.
- Key Findings: TPC spectra identified two distinct defect energy thresholds at 1.2 eV (vacancy or NV center related) and 2.2 eV (attributed to NV centers). Charge state transitions (NV+ → NV0 → NV-) were actively controlled by applying reverse bias voltages from 0 V to -30 V.
- Photocapacitance Dynamics: Steady-state photocapacitance measurements revealed that applying reverse bias drastically reduces trap filling time from >20 minutes (at 0 V) to approximately 12 seconds.
- Technological Impact: Demonstrates a viable pathway for developing quantum devices requiring precise, electrically addressable NV centers within a wide bandgap (5.5 eV) semiconductor matrix.
Technical Specifications
Section titled “Technical Specifications”| Parameter | Value | Unit | Context |
|---|---|---|---|
| Substrate Material | IIb HPHT Diamond (001) | — | Off-angle of 3.5° |
| Epitaxial Layer Thickness | 1 | µm | Boron-doped homoepitaxial layer |
| Epitaxial Layer Doping | 3 × 1016 | cm-3 | Slightly boron-doped |
| Growth Method | MPCVD | — | Homoepitaxial growth |
| Ion Implantation Energy | 80 | keV | Nitrogen ions |
| Mean Implantation Depth | ~100 | nm | Calculated via SRIM simulation |
| Implantation Dose | 1012 | ions/cm2 | Nitrogen ions |
| Implantation Temperature | 600 | °C | Elevated temperature process |
| Annealing Temperature | 1000 | °C | For NV center formation |
| Annealing Duration | 1 | hour | In inert/forming gas |
| Schottky Electrode Material | Molybdenum (Mo) | — | 10 nm thick, 300 µm diameter |
| Ohmic Electrode Stack | Ti (30 nm) / Pt (30 nm) / Au (100 nm) | — | Backside contact |
| Ohmic Contact Annealing | 420 | °C | 30 minutes, forming titanium carbide |
| Defect Energy Level 1 | 1.2 | eV | Identified via TPC (Vacancy/NV related) |
| Defect Energy Level 2 | 2.2 | eV | Identified via TPC (NV center related) |
| Photocapacitance Decay Time (0 V) | > 20 | minutes | Trap filling time under 564 nm illumination |
| Photocapacitance Decay Time (Reverse Bias) | ~12 | seconds | Trap filling time under reverse bias |
| NV0 ZPL Wavelength | 575 | nm | Characteristic photoluminescence peak |
| NV- ZPL Wavelength | 637 | nm | Characteristic photoluminescence peak |
| Trap Density (Nt) | ~1015 | cm-3 | Estimated from steady-state photocapacitance |
| Photoionization Cross-section | ~10-15 | cm2 | Estimated for 2.2 eV defect |
| Ideality Factor (Non-implanted) | 1.8 | — | Diode parameter |
| Ideality Factor (Implanted) | 2.8 | — | Diode parameter |
| Dark Saturation Current (Non-implanted) | 7.9 × 10-14 | A | Diode parameter |
| Reverse Bias Range | 0 to -30 | V | For charge state control |
Key Methodologies
Section titled “Key Methodologies”- Substrate Preparation: Utilization of IIb HPHT (001) diamond substrates with a 3.5° off-angle to facilitate high-quality epitaxial growth.
- Epitaxial Growth: Deposition of a 1 µm thick slightly boron-doped (3 × 1016 cm-3) diamond layer via MPCVD.
- Ion Implantation: Half of the sample subjected to nitrogen ion implantation at 80 keV with a dose of 1012 ions/cm2 at an elevated temperature of 600 °C to control defect distributions.
- Thermal Annealing: Post-implantation annealing at 1000 °C for 1 hour to mobilize vacancies and form stable NV centers.
- Surface Treatment: UV ozone treatment prior to Schottky contact deposition to create an oxygen-terminated diamond surface.
- Ohmic Contact Fabrication: Photolithographic deposition of Ti (30 nm) / Pt (30 nm) / Au (100 nm) on the backside, followed by 420 °C annealing for 30 minutes to form titanium carbide.
- Schottky Contact Fabrication: Deposition of 10 nm Mo electrodes (300 µm diameter) using a photolithography sandwich structure technique.
- TPC Spectroscopy: Utilization of a Boonton 72B capacitance meter (1 MHz frequency) with a halogen lamp (400-1200 nm) and a quiescent reverse bias combined with a 500 ms filling pulse (0 V, 10 s duration).
- PL Spectroscopy: Measurement under different applied bias conditions (0 V to -30 V) using a 532 nm green laser at room temperature.
- Steady-State Photocapacitance: Illumination with a 564 nm wavelength light source to monitor charge trap dynamics over time.
6CCVD Solutions & Capabilities
Section titled “6CCVD Solutions & Capabilities”To replicate, validate, or extend the findings of this research on electrically controlled NV centers in diamond Schottky diodes, specific high-quality materials and customization services are required. 6CCVD provides the necessary infrastructure to support this advanced quantum device research.
Applicable Materials
Section titled “Applicable Materials”- Optical Grade Single Crystal Diamond (SCD): The paper relies on a IIb HPHT diamond substrate overgrown with a high-purity, low-defect homoepitaxial layer. 6CCVD provides Optical Grade SCD wafers and substrates up to 125mm, ensuring the low background impurity levels required for sensitive TPC and PL spectroscopy.
- Slightly Boron-Doped Diamond: The active layer requires precise doping control (3 × 1016 cm-3). 6CCVD specializes in custom MPCVD epitaxial growth with tailored boron concentrations to engineer the desired carrier density and depletion region widths.
- Polycrystalline Diamond (PCD): For applications requiring larger active areas or high-throughput device fabrication, 6CCVD offers custom PCD plates that can be processed and evaluated for similar NV center charge control experiments.
Customization Potential
Section titled “Customization Potential”- Custom Metalization: The paper utilizes a specific Ti/Pt/Au (30/30/100 nm) Ohmic stack and a Mo (10 nm) Schottky contact. 6CCVD offers in-house metalization capabilities including Au, Pt, Pd, Ti, W, and Cu, allowing for exact replication of these contact architectures or optimization for alternative Schottky barrier heights.
- Laser Cutting & Shaping: The 300 µm diameter Mo electrodes were defined via photolithography. 6CCVD provides precise laser cutting and structuring services to fabricate custom electrode geometries and die sizes from bulk diamond material.
- Thickness Control: The 1 µm epitaxial layer was critical for the depletion region interaction with the NV centers. 6CCVD offers precise thickness control for SCD/PCD layers ranging from 0.1 µm to 500 µm to match specific device depth requirements.
Engineering Support
Section titled “Engineering Support”- Application-Specific Consultation: Developing quantum devices based on NV centers requires a deep understanding of defect engineering, Fermi level positioning, and charge state dynamics. 6CCVD’s in-house PhD engineering team can assist with material selection, doping calibration, and architecture design for quantum sensing and quantum computing projects.
- Process Optimization: Whether the goal is maximizing NV creation efficiency during implantation or tuning the photocapacitance response, our team can provide guidance on material parameters that influence trap density and carrier lifetimes.
Call to Action
Section titled “Call to Action”The successful demonstration of electrical control over NV center charge states is a critical milestone for next-generation quantum technologies. To achieve reproducible results, the quality of the diamond substrate and epitaxial layer is paramount. 6CCVD is equipped to supply the precise, high-purity diamond materials and custom metalization required to advance this research.
For custom specifications or material consultation, visit 6ccvd.com or contact our engineering team directly.
View Original Abstract
Abstract The study of nitrogen-vacancy (NV) centers in diamond are growing attractive in the application of quantum devices. Here, electrical control of NV charge state and defects induced by nitrogen ions implantation in diamond were investigated by transient photocapacitance (TPC) spectroscopy and photoluminescence (PL) spectroscopy. The experiments show that thresholds of 1.2 eV appeared in TPC spectra are probably due to the presence of excited defect energy levels related to vacancy or NV center. Alternatively, the 2.2 eV defect observed in the TPC spectrum is probably attributed to NV centers. The variation of TPC and PL spectra with different applied voltages suggests that bias voltages control the charge state of NV centers since their effect on the Fermi level shifting in the depletion region. Furthermore, the steady-state photocapacitance indicates that the 2.2 eV deep trap slows down the process of photocapacitance rise and fall, and these processes can be enhanced by a higher electrical field.