Thermally Stimulated and Dynamic Effects in Identification and Study of Carbon Materials by Raman Spectroscopy
At a Glance
Section titled “At a Glance”| Metadata | Details |
|---|---|
| Publication Date | 2021-01-01 |
| Journal | Učënye zapiski Kazanskogo universiteta. Seriâ Estestvennye nauki/Učënye zapiski Kazanskogo universiteta. Seriâ Estestvennye nauki/Učenye zapiski Kazanskogo gosudarstvennogo universiteta. Seriâ Estestvennye nauki |
| Authors | С. И. Исаенко, Т. Г. Шумилова |
| Institutions | Russian Academy of Sciences, Institute of Geology, Komi Science Centre |
| Citations | 3 |
| Analysis | Full AI Review Included |
Executive Summary
Section titled “Executive Summary”- Core Focus: Analysis of thermally stimulated and dynamic effects in Raman spectroscopy when applied to carbon materials (graphite, glassy carbon, SCD, lonsdaleite, ultrananocrystalline diamond).
- Critical Finding: Laser-induced heating causes significant “red shift” (downshift) of diagnostic Raman lines, which can lead to misinterpretation of spectra or complete sample combustion.
- Particle Size Thresholds: Thermal effects become pronounced for graphite particles < 4 µm, SCD fragments ≤ 1 µm, and nanocrystalline/ultrananocrystalline diamond particles ≤ 10 µm.
- Diamond T2g Mode Stability: The 1332 cm-1 peak shifts by -0.012 cm-1/K and -0.011 cm-1/K (graphite G-band), confirmed up to 1900 K.
- Novel Application: Controlled laser heating (> 10 mW at 488 nm) was used to thermally ablate glassy carbon shells, exposing underlying nanocrystalline diamond cores (togorite samples).
- Methodology: LabRam HR800 confocal micro-Raman with 488 nm, 514.5 nm, and 632.8 nm laser excitation, neutral density filters (10×, 100×, 1000× attenuation), and 0.1-200 mW power range.
- Key Achievement: Established practical power limits for safe spectral acquisition of micro- and nano-sized carbon particles without causing phase transformation or combustion.
Technical Specifications
Section titled “Technical Specifications”| Parameter | Value | Unit | Context |
|---|---|---|---|
| Diamond T2g reference position | 1332 | cm-1 | Standard conditions (sp3 carbon) |
| Graphite G-band reference position | 1582 | cm-1 | Highly crystalline graphite, E2g(2) mode |
| Diamond thermal shift coefficient | -0.012 | cm-1/K | Line shift per degree temperature increase |
| Graphite G-band thermal shift coefficient | -0.011 | cm-1/K | HOPG reference data |
| Diamond pressure shift coefficient | 2.2 | cm-1/GPa | Hydrostatic pressure dependence |
| Graphite G-band pressure shift coefficient | 4.7 | cm-1/GPa | Hydrostatic pressure dependence |
| Maximum G-band shift (glass carbon) | 17 | cm-1 | Observed at 200 mW (514.5 nm) |
| Maximum D-band shift (glass carbon) | 13 | cm-1 | Observed at 200 mW (514.5 nm) |
| Maximum G-band shift (graphite particles 1-4 µm) | 11-12 | cm-1 | At max laser power |
| Maximum G-band shift (togorite shell) | 18 | cm-1 | Corresponds to ~1900 K |
| Maximum diamond line shift (togorite core) | 10 | cm-1 | Corresponds to ~1100 K |
| Diamond SCD induced heating (10 mW, 1 µm) | 217 | K | Calculated from 2.6 cm-1 shift |
| Raman instrument used | LabRam HR800 | — | Horiba Jobin Yvon, confocal |
| Grating densities | 600, 1800 | lines/mm | Spectrograph configuration |
| Confocal hole sizes | 300, 500 | µm | Aperture settings |
| Spectrometer slit | 100 | µm | Entrance slit width |
| Objectives | ×50, ×100 | — | Magnification |
| Laser 1 (He-Ne) | 632.8 | nm | Pmax = 20 mW |
| Laser 2 (Ar+) | 488 / 514.5 | nm | Pmax = 200 mW |
| Exposure time | 1-30 | s | Per spectral acquisition |
| Accumulation cycles | 10 | — | Signal averaging |
| Density filters | D1, D2, D3 | — | 10×, 100×, 1000× attenuation |
| Critical particle size (graphite) | < 4 | µm | Laser heating threshold |
| Critical particle size (SCD) | ≤ 1 | µm | Combustion threshold at 100 mW |
| Critical particle size (UNCD/NCD) | ≤ 10 | µm | Maximum red shift observed |
| D-band typical range | 1330-1360 | cm-1 | Disorder-activated mode |
| Diamond FWHM after shell burn | 13-16 | cm-1 | At 0.1-10 mW |
| Lonsdaleite crystallite size (togorite) | 20-30 | nm | Nanocrystalline regime |
Key Methodologies
Section titled “Key Methodologies”- Sample Preparation: Natural and synthetic carbon phases (Ceylon graphite, SU-2000 glassy carbon, A380/63 synthetic diamond, Kumdykol lonsdaleite, Kara astrobleme impactites) were prepared via thermochemical decomposition using H2SO4/K2Cr2O7 oxidation, NaOH fusion at 500 °C, and distilled water leaching.
- Instrumentation Setup: LabRam HR800 confocal micro-Raman spectrometer with ×50/×100 objectives, 600/1800 lines/mm gratings, 100 µm slit, and 300/500 µm confocal pinholes.
- Laser Excitation: Three wavelengths tested: 632.8 nm (He-Ne, 20 mW max), 514.5 nm and 488 nm (Ar+, 200 mW max).
- Power Attenuation: Neutral density filters (D1, D2, D3) applied in 10× reduction steps (10×, 100×, 1000×) to control sample heating.
- Acquisition Parameters: Exposure times of 1-30 s with 10 accumulation cycles for signal-to-noise optimization.
- Controlled Heating Protocol: Power was systematically stepped from 0.1 mW → 1 mW → 10 mW → 100 mW while monitoring spectral shifts.
- Dynamic Registration Technique: For lonsdaleite detection, initial spectrum at 1 mW followed by rapid sequential acquisitions at 10 mW to induce near-critical thermal conditions.
- Shell-Burn Method: 488 nm laser at 10 mW applied continuously for 6-25 minutes to thermally ablate glassy carbon shells and expose nanocrystalline diamond cores.
- Spectral Deconvolution: Gaussian-Lorentzian fitting in LabSpec 5.39 software used to resolve overlapping D, G, and T2g bands.
- Calibration Standards: Reference values of 1332 cm-1 (diamond) and 1582 cm-1 (graphite) at standard temperature and pressure.
6CCVD Solutions & Capabilities
Section titled “6CCVD Solutions & Capabilities”-
Applicable Materials:
- Optical Grade Single Crystal Diamond (SCD): The T2g mode at 1332 cm-1 requires ultra-low impurity SCD with FWHM < 2 cm-1 for accurate Raman thermometry. 6CCVD provides optical-grade SCD plates with thickness from 0.1 µm to 500 µm and surface roughness Ra < 1 nm, ideal for thermal characterization studies.
- Polycrystalline Diamond (PCD): For nanocrystalline/ultrananocrystalline diamond investigations, 6CCVD’s PCD substrates (up to 10 mm thickness) up to 125 mm diameter offer well-defined reference samples with controlled grain boundaries.
- Boron-Doped Diamond (BDD): For stress/strain mapping experiments where electrical conductivity is needed, our BDD films enable in situ Raman measurements under applied bias or current.
-
Customization Potential:
- Laser-Compatible Geometry: The paper’s micron-scale particle analysis demands precisely cut substrates. 6CCVD offers laser cutting and custom dicing to deliver SCD/PCD squares, rectangles, or complex geometries down to sub-millimeter dimensions.
- Metallization for Thermal Management: Researchers studying laser-induced heating can benefit from 6CCVD’s internal metallization capabilities (Ti, Pt, Au, W, Cu) to create heat-spreading layers or reflective coatings that mitigate thermal artifacts during high-power Raman acquisition.
- Polished Windows: Both surfaces can be polished to Ra < 1 nm (SCD) or < 5 nm (inch-size PCD) to minimize background scattering and ensure confocal Raman accuracy.
-
Engineering Support:
- Application-Specific Consultation: 6CCVD’s in-house PhD team can assist with material selection for Raman spectroscopy calibration standards, thermal conductivity benchmarks, and high-pressure diamond anvil cell (DAC) experiments.
- Reference Sample Provision: Need a stable Raman reference (1332 cm-1 ± 0.5 cm-1)? We can deliver certified SCD standards with documented spectral fingerprints.
- Diamond Anvil Cell Material: For high-pressure Raman studies like those cited (Akahama, Hanfland), 6CCVD’s optical-grade SCD anvils provide the mechanical durability and optical transparency required for multi-MPa pressure-temperature investigations.
-
Call to Action: For custom specifications or material consultation, visit 6ccvd.com or contact our engineering team directly.
View Original Abstract
In this paper, the aspects of studying micron-sized carbon material substances using Raman spectroscopy with laser excitation were discussed. The relevance of the study is determined by the fact that the positions of diagnostic lines in the Raman spectra of carbon materials are significantly affected as the analyzed sample region is heated during the process of spectra recording, thereby resulting in a shift of the diagnostic lines and bands, up to the burnout of the analyzed particle region or to the complete combustion of the sample. To assess the influence of the laser radiation power on the position of diagnostic lines in the Raman spectra of carbon materials, we studied the position of the lines depending on the laser power and sample size of both natural and man-made carbon phases of various structures: highly crystalline graphite, glassy carbon, cubic monocrystalline diamond, hexagonal monocrystalline diamond (lonsdaleite), and ultrananocrystalline diamond. The study was performed by Raman spectroscopy with the use of a high-resolution LabRam HR800 microspectrometer (Horiba, Jobin Yvon). For mono-, nano-, and ultrananocrystalline diamonds, a number of examples were provided to demonstrate that the exciting laser power during Raman spectroscopy measurements of carbon materials must be especially carefully monitored in particles of 10 μm or less in size. For highly crystalline graphite particles, the laser power must be controlled in samples smaller than 4 μm in size. When the Raman spectra were registered during the controlled laser heating, it was found that the samples of a black carbon variety between coal and diamond (described as togorite by V.A. Yezersky V.A. (1986)) had intergrowths of diamond and glassy carbon, a diamond core with a glass-like carbon shell. The results obtained show that the controlled use of the thermal effect of laser radiation can be helpful in identification of the detailed spectroscopic characteristics that occur during the intensive heating of samples, as well as in recovering mineral individuals from aggregates.