Large Area Diamond Disk Growth Experiments and Thermomechanical Investigations for the Broadband Brewster Window in DEMO

MetadataDetails
Publication Date2021-06-22
JournalIEEE Transactions on Electron Devices
AuthorsG. Aiello, Konstantinos A. Avramidis, T. Franke, G. Gantenbein, John Jelonnek
InstitutionsDiamond Materials (Germany), Karlsruhe Institute of Technology
Citations11
AnalysisFull AI Review Included
  • Core Breakthrough: Successful growth and characterization of the first worldwide free-standing optical-grade CVD diamond disk measuring Ø180 mm, surpassing the previous state-of-the-art of 140 mm.
  • Target Application: Broadband Brewster-angle RF window for the European DEMO fusion reactor’s Electron Cyclotron System (ECS), specifically designed for 2 MW frequency step-tunable gyrotrons.
  • Operational Frequencies: Designed for dual-frequency operation at 170 GHz and 204 GHz, with extended bandwidths up to ~238 GHz.
  • Disk Geometry: Average unpolished thickness of 1.3 mm, optimized for the Brewster angle of 67.2° for diamond (refractive index ~2.47).
  • Dielectric Performance: Loss tangent (tan δ) measurements conducted at the center and over large areas on a one-sided polished disk, showing values suitable for high-power CW operation.
  • Thermal Management: Integrated water cooling channels in pure copper housings (upper/lower channel covers) to manage thermal loads from MW-class microwave beams.
  • Method Validation: Comprehensive thermomechanical simulations confirming structural integrity and thermal distribution under CW gyrotron operation scenarios.
ParameterValueUnitContext
Disk Diameter180mmFree-standing optical-grade CVD diamond
Disk Thickness (unpolished avg.)1.3mmOptimized for Brewster-angle window
Brewster Angle (diamond)67.2°Angle for zero reflection at diamond interface
Operating Frequency 1170GHzMain gyrotron frequency for DEMO
Operating Frequency 2204GHzSecondary gyrotron frequency
Extended Frequency~238GHzFuture frequency tuning range
Microwave Power2MWOutput gyrotron power (CW)
Waveguide Inner Diameter63.5mmCorrugated HE11 waveguide aperture
Frequency Tuning Range±10GHzStep-tunable around center frequencies
Loss Tangent (tan δ)2.7×10⁻⁶ (min) to 1.3×10⁻⁵—Measured across disk area
Diamond Thermal Conductivity>1800W/(m·K)Typical for optical-grade CVD diamond
Cooling Water Flow Rate (tested)12-42L/minInlet manifold flow range
Housing MaterialPure Copper—Upper/lower channel covers for brazed assembly
  1. Diamond Growth: Microwave Plasma Chemical Vapor Deposition (MPCVD) performed by Diamond Materials GmbH to achieve Ø180 mm free-standing optical-grade diamond.
  2. Surface Polishing: One side of the large-area disk was polished to optical grade for dielectric property characterization.
  3. Loss Tangent Characterization: Measurements performed at the disk center and over a large spatial area to verify homogeneity of dielectric properties.
  4. Thermomechanical Analysis (FEA): Consistent set of simulations evaluating thermal gradients, stress distributions, and displacements under CW gyrotron loading.
  5. Cooling Channel Design: Pure copper housing with integrated upper/lower channel covers and inlet/outlet manifolds for forced water cooling.
  6. Brazing Assembly: Diamond disk brazed into the copper waveguide housing using appropriate brazing alloys to ensure vacuum integrity.
  7. Parametric Cooling Study: Flow rate variation (12-42 L/min) analyzed to optimize thermal management at 204 GHz and 238 GHz operating conditions.
  8. Structural Support: Fixed support boundary conditions applied at the housing periphery, with the CVD diamond disk bonded via brazing interfaces.
  • Optical-Grade SCD (Single Crystal Diamond): While this paper utilized Polycrystalline CVD diamond, 6CCVD’s optical-grade SCD and high-quality PCD are ideal for Brewster-angle window applications requiring ultra-low loss tangents and high thermal conductivity.
  • Large-Area PCD Plates: 6CCVD offers polycrystalline diamond plates with custom dimensions up to 125 mm (PCD), with the capability to discuss larger formats for fusion and high-power microwave applications.
  • Optical Polishing Services: 6CCVD provides Ra < 1 nm polishing for SCD and < 5 nm for inch-size PCD, essential for minimizing surface scattering losses in gyrotron window applications.
  • Custom Thickness Control: The 1.3 mm disk thickness demonstrated here aligns with 6CCVD’s SCD/PCD thickness range of 0.1 µm - 500 µm, with substrates available up to 10 mm for thicker Brewster-window geometries.
  • Metalization for Brazing: 6CCVD’s in-house metalization capabilities (Au, Pt, Pd, Ti, W, Cu) are directly applicable for the Ti-based brazing interfaces used to bond diamond disks into copper waveguide housings. Custom metal stacks can be tailored to match coefficient-of-thermal-expansion (CTE) requirements.
  • Laser Cutting & Shaping: Non-standard disk geometries (e.g., elliptical apertures for Brewster-angle mounting) can be achieved through 6CCVD’s precision laser cutting services.
  • Brazing-Ready Surfaces: Optional surface metallization and pre-treatment to facilitate integration with copper or Glidcop® housings.
  • PhD-Level Consultation: 6CCVD’s in-house PhD engineering team can assist with material selection, loss tangent optimization, and thermomechanical modeling for high-power microwave window projects.
  • Application-Specific Guidance: For fusion, plasma physics, and high-power gyrotron applications, our engineers can recommend optimal grain size, doping levels, and surface finishes.
  • Diamond-to-Metal Joining Expertise: Guidance on compatible metallization schemes for vacuum-tight brazing of diamond into waveguide assemblies.

For custom specifications, material consultation, or to discuss large-area optical-grade diamond for fusion and high-power microwave applications, visit 6ccvd.com or contact our engineering team directly.

View Original Abstract

An electron cyclotron system (ECS) is required in the European DEMO fusion reactor for plasma heating, magnetohydrodynamic control, especially the suppression of neoclassical tearing modes (NTMs), and thermal instability control. Microwave beams of 2 MW, generated by gyrotrons, shall propagate through corrugated HE 11 waveguides (WGs) of 63.5-mm inner diameter and finally reach specific locations in the plasma by a dedicated set of mirrors. The deployment of the beam may be done either by angular steering, i.e., tilting moveable mirrors, or by frequency steering, i.e., tuning the gyrotron frequency. In the last option, for long pulse operations, broadband optical grade diamond windows are required as confinement and/or vacuum barriers both at the torus and the gyrotron side. The Brewster-angle window represents a promising solution due to its intrinsic simplicity. However, the WG aperture imposes a minimum Ø180 mm for the disk at the Brewster-angle of 67.2° for diamond. This is an ambitious target, considering 140 mm as the state of the art. First, this article shows the very promising results of diamond growth experiments carried out by Diamond Materials GmbH with the first worldwide free-standing optical grade Ø180-mm disk having an average unpolished thickness of 1.3 mm. For the first time, one side of this large disk was polished and loss tangent measurements were performed at the center and over a large area. Then, the performance of the window featuring these large disks was characterized by a consistent set of thermomechanical analyses in view of the forthcoming window prototyping activity.

  1. 2016 - Properties of diamond produced by chemical vapor deposition process for ITER diagnostic window assembly applications