Magnetically sensitive fiber probe with nitrogen-vacancy center nanodiamonds integrated in a suspended core
At a Glance
Section titled “At a Glance”| Metadata | Details |
|---|---|
| Publication Date | 2022-05-03 |
| Journal | Optics Express |
| Authors | Adam Filipkowski, Mariusz Mrózek, Grzegorz Stępniewski, Maciej J. Głowacki, Dariusz Pysz |
| Institutions | Institute of Microelectronics, Gdańsk University of Technology |
| Citations | 15 |
| Analysis | Full AI Review Included |
Executive Summary
Section titled “Executive Summary”- Core Innovation: Development of a suspended-core silicate glass fiber with 750 nm nitrogen-vacancy (NV-) nanodiamonds centrally embedded within a 1.5 µm solid glass core for distributed magnetometry.
- Method: Two-stage fiber drawing process using low-melting-point F2 lead silicate glass (Tg1 = 434°C) in nitrogen atmosphere to prevent diamond graphitization, combined with dip-coating deposition of nanodiamonds at sub-600°C processing temperatures.
- Geometry: Core-to-particle diameter ratio of 2:1 ensures nanodiamonds overlap directly with the guided optical mode, maximizing fluorescence coupling.
- Performance: Achieved 7% ODMR readout contrast and magnetic field sensitivity of 0.5 µT·Hz-1/2—two orders of magnitude improvement over prior fiber-integrated NV sensor designs.
- Validation: Tested on a 24 cm-long fiber sample with 532 nm laser excitation and microwave loop gap antenna resonant driving.
- Application Scope: Magnetic field mapping, gradiometry, biosensing, and microfluidic implementations leveraging intrinsic air channels.
Technical Specifications
Section titled “Technical Specifications”| Parameter | Value | Unit | Context |
|---|---|---|---|
| Mean nanodiamond diameter | 750 | nm | MDNV1um grade, Adámas Nanotechnologies |
| Fiber core diameter | ~1.5 | µm | Suspended core, solid glass |
| Core-to-particle ratio | 2:1 | - | Ensures direct mode overlap |
| Bridge thickness (suspended struts) | 150-280 | nm | Three struts supporting core |
| Final fiber outer diameter | ~125 | µm | Standard fiber format |
| Sub-preform outer diameter | 3.7 | mm | Intermediate draw stage |
| Core glass transition temp (Tg1) | 434 | °C | Schott F2 lead silicate |
| Cladding glass transition temp (Tg2) | 445 | °C | Modified F2-like composition |
| Draw temperature range | 710-760 | °C | Nitrogen atmosphere |
| Preform burn-off temperature | 400 | °C | Oxygen atmosphere (dust removal) |
| Core refractive index (n1, 589.3 nm) | 1.6199 | - | F2 lead silicate |
| Cladding refractive index (n2, 589.3 nm) | 1.6133 | - | Modified F2-like glass |
| Diamond suspension concentration | 0.05 | % | Ethanol-based dip-coating |
| Diamond oxidation/graphitization limit | 600 | °C | Process ceiling constraint |
| Fiber length tested | 24 | cm | Proof-of-concept ODMR sample |
| ODMR readout contrast | ~7 | % | Suspended core design |
| Magnetic field sensitivity | 0.5 | µT·Hz-1/2 | Guided mode readout |
| Sensitivity improvement vs. prior | ~100× | - | Compared to earlier fiber designs |
| Excitation wavelength | 532 | nm | Green laser pump |
| Reference prior ODMR contrast | 3.5 / 2.5 / ~1 | % | Tellurite / silicate ring / stacked cane designs |
Key Methodologies
Section titled “Key Methodologies”- Glass Selection: Schott F2 lead silicate core glass (Tg1 = 434°C) selected for low draw temperature compatibility with diamond particles; modified F2-like cladding glass melted in-house (Tg2 = 445°C).
- Nanodiamond Deposition: Dip-coating protocol using 750 nm diamond suspension in ethanol at 0.05% concentration inside F2 glass tube (dc1 = 3.4 mm, dc2 = 2.4 mm), repeated 10× with drying between cycles.
- First-Stage Draw: Dip-coated tube collapsed and drawn to dc = 0.3 mm at 710-760°C in nitrogen atmosphere to prevent graphitization; 400°C oxygen pre-treatment for dust removal.
- Preform Assembly: Three glass capillaries (dt2 = 7.4 mm) arranged triangularly inside a 16 mm inner-diameter tube, interstitial spaces filled with low-index rods, with the nanodiamond-loaded core cane inserted centrally.
- Second-Stage Draw: Sub-preform drawn to ds = 3.7 mm with equalized hole pressure to prevent clogging; core capillary collapsed to embed nanodiamonds at the geometric center.
- Final Fiber Draw: Equal pressure applied across three air channels to form suspended-core microstructure with thin glass bridges (150-280 nm).
- ODMR Characterization: 532 nm laser excitation through microscope objective; microwave driving via loop gap antenna; fluorescence collected from far fiber end as guided mode through dichroic filter and spectrometer.
- Magnetic Sensitivity Measurement: Allan deviation analysis on 24 cm fiber sample yielding 0.5 µT·Hz-1/2 sensitivity.
6CCVD Solutions & Capabilities
Section titled “6CCVD Solutions & Capabilities”Applicable Materials
Section titled “Applicable Materials”The research relies on nitrogen-vacancy (NV-) ensembles in nanodiamond particles with controlled size (~750 nm) and stable fluorescence. For replication or extension of this work:
| Application Requirement | Recommended 6CCVD Material |
|---|---|
| NV- ensemble nanodiamonds (sub-µm) | Optical Grade SCD particles or detonation nanodiamond aggregates (custom size classification available) |
| Bulk diamond reference / alternative geometry | Optical Grade SCD plates/wafers for fiber-tip magnetometry variants |
| Enhanced NV- concentration | High-Nitrogen SCD or irradiation-treated SCD for controlled defect engineering |
| Electrochemical / biosensor variants | Boron-Doped Diamond (BDD) with tunable conductivity |
Customization Potential
Section titled “Customization Potential”- Sub-µm Particle Sizing: 6CCVD provides custom size-classified nanodiamond fractions from bulk SCD feedstock—essential for next-generation designs where smaller particles (as the authors note) would reduce scattering losses and improve homogeneity.
- Custom Substrate Geometry: While this paper used glass host matrices, 6CCVD can supply freestanding SCD membranes (0.1 µm - 500 µm) for alternative fiber-tip or waveguide-integrated sensor architectures.
- Metalization Services: For hybrid fiber probes requiring metallized diamond elements (antenna coupling, plasmonic enhancement, or electrical readout), 6CCVD offers in-house deposition of Ti, Pt, Au, Pd, W, and Cu with sub-µm patterning capability.
- Laser Cutting & Dicing: Custom shaping of diamond elements to micron precision for integration into microstructured fiber preforms.
- Surface Functionalization: Polished surfaces (Ra < 1 nm for SCD, < 5 nm for inch-size PCD) suitable for chemical functionalization, biomarker attachment, or van der Waals integration onto fiber tapers.
Engineering Support
Section titled “Engineering Support”This paper highlights several engineering challenges that 6CCVD’s in-house PhD team can address:
- Particle Size Optimization: Smaller, more uniform nanodiamond fractions reduce propagation loss and improve NV- fluorescence homogeneity along extended fiber lengths.
- NV- Yield Enhancement: Custom nitrogen doping profiles and post-growth irradiation/annealing protocols to maximize NV- formation yield per particle.
- Diamond-Polymer vs. Diamond-Glass Integration: For gradiometer or biosensor variants requiring flexible hosts, 6CCVD can advise on diamond particle integration strategies.
- Cryogenic Compatibility: For pulse-protocol implementations (spin-echo, dynamical decoupling) the authors recommend, low-temperature NV- coherence data is available for material selection guidance.
Project Consultation Available: 6CCVD’s engineering team supports NV-diamond magnetometry, quantum sensing, and biomedical diagnostic programs from material selection through prototype delivery.
For custom specifications or material consultation, visit 6ccvd.com or contact our engineering team directly.
View Original Abstract
Efficient collection of photoluminescence arising from spin dynamics of nitrogen vacancy (NV) centers in diamond is important for practical applications involving precise magnetic field or temperature mapping. These goals may be realized by the integration of nanodiamond particles with optical fibers and volumetric doping of the particles alongside the fiber core. That approach combines the advantages of robust axial fixation of NV diamonds with a direct spatial overlap of their fluorescence with the guided mode of the fiber. We developed a suspended core silicate glass fiber with 750 nm-diameter nanodiamonds located centrally in the 1.5 µm-core cross-section along its axis. The developed fiber probe was tested for its magnetic sensing performance in optically detected magnetic resonance measurements using a 24 cm-long fiber sample, with the NV excitation and fluorescence collection from the far ends of the sample and yielding optical readout contrast of 7% resulting in 0.5 µT·Hz -1/2 magnetic field sensitivity, two orders of magnitude better than in earlier designs. Thanks to its improved fluorescence confinement, the developed probe could find application in magnetic sensing over extended fiber length, magnetic field mapping or gradiometry.