Skip to content

Observation of chip-producing behavior in ultraprecision diamond cutting of additively manufactured Alloy 718 utilizing ultrasonic elliptical vibration

MetadataDetails
Publication Date2024-01-01
JournalJournal of Advanced Mechanical Design Systems and Manufacturing
AuthorsS. Kawasaki, Norio Yamashita, Shinya Morita, Hideo Yokota
InstitutionsRIKEN Center for Advanced Photonics, Tokyo Denki University
AnalysisFull AI Review Included
  • Breakthrough in Difficult-to-Cut Materials: Achieved ultraprecision mirror-surface machining of additively manufactured (AM) Alloy 718 using Ultrasonic Elliptical Vibration Cutting (UEVC) with a single-crystal diamond (SCD) flat tool.
  • Nanometer-Level Surface Finish: Attained a minimum surface roughness Ra of 8.4 nm at a cutting speed of 2.0 mm/s, pushing below the 10 nm mirror-surface threshold previously considered a major challenge for Ni-based superalloys.
  • Stable Ductile-Regime Cutting: Flow-type chip formation was consistently observed across all cutting speeds (0.5-5.0 mm/s), vibration amplitudes (1.0-4.0 µmp-p), and depth-of-cut conditions (1-3 µm), confirming predictable, stable material removal.
  • Superior SCD Tool Life: The SCD cutting edge retained a mirror surface with only slight wear over a cutting distance of approximately 50 m—significantly extending feasible cutting distances compared to conventional diamond turning of Inconel-family alloys.
  • Dry, Eco-Friendly Process: The lubrication-free UEVC method reduces environmental impact and operational costs while suppressing heat generation at the tool-workpiece interface, mitigating carbon diffusion and chemical degradation of the diamond.
  • Method Validation: The approach was demonstrated on SLM-built Alloy 718 with fine columnar grain microstructures, validating the technique for next-generation aerospace and gas turbine components.
ParameterValueUnitContext
Workpiece MaterialAlloy 718 (Inconel 718)—Additively manufactured via Selective Laser Melting (SLM)
Tool TypeSingle-Crystal Diamond (SCD), flat-edged—UPC series, A.L.M.T. Corp.
Rake Angle0°Flat-faced geometry
Clearance Angle12°Standard UEVC geometry
Cutting Edge Width1.0mmLinear planar contact
Cutting Speed Range0.5 - 5.0mm/sVariable parameter
Optimal Cutting Speed2.0mm/sBest Ra result
Vibration Amplitude Range1.0 - 4.0µmp-pElliptical vibration
Depth of Cut Range1 - 3µmMicro-cutting regime
Minimum Surface Roughness (Ra)8.4nmAchieved at 2.0 mm/s
Maximum Surface Roughness (Rz)~70nmAt lowest amplitude (1.0 µmp-p)
Chip Thickness (max)~1.5µmAt 1.0 µmp-p amplitude
Demonstrated Tool Life~50mMirror-edge wear onset
UEVC DeviceEL-50Σ (Taga Electric)—40 kHz ultrasonic system
Positioning Repeatability< 1.0µmRiken Micro Slicer System 004
  1. Sample Preparation: AM Alloy 718 test coupons produced by Selective Laser Melting (SLM), exhibiting characteristic fine columnar grain microstructures.
  2. Tool Selection: Single-crystal diamond (SCD) flat tool with 0° rake angle, 12° clearance angle, and 1.0 mm cutting edge width—chosen over PCD for superior edge sharpness despite traditional wear concerns.
  3. UEVC Setup: Ultrasonic elliptical vibration device (EL-50Σ, Taga Electric) mounted on the Riken Micro Slicer System 004 (RMSS-004) with sub-micron positioning repeatability.
  4. Planar Cutting Execution: Single-stroke planar cuts applied across a parameter matrix:
    • Cutting speed: 0.5, 1.0, 2.0, 3.0, 4.0, 5.0 mm/s
    • Vibration amplitude: 1.0, 1.5, 2.0, 2.5, 3.0, 4.0 µmp-p
    • Depth of cut: 1, 2, 3 µm
  5. Surface Evaluation: Surface roughness (Ra, Rz) measured with on-board optical metrology (Mitutoyo M Plan Apo objective + Olympus PEN-F digital capture).
  6. Chip Morphology Analysis: Scanning Electron Microscopy (SEM) used to characterize chip geometry and thickness, confirming flow-type (ductile-regime) chip formation.
  7. Tool Wear Assessment: Cutting edge inspected over extended cutting distances (~50 m) to determine feasible service life under UEVC conditions.
  8. Dry Machining: All experiments conducted without lubricant, leveraging UEVC’s intrinsic heat-suppression mechanism.

Applicable Materials:

The research relies on a high-purity, defect-free Single-Crystal Diamond (SCD) cutting tool with a precisely oriented 1.0 mm flat cutting edge. 6CCVD manufactures Optical-Grade SCD substrates and freestanding plates using Microwave Plasma Chemical Vapor Deposition (MPCVD), offering:

  • SCD thickness range: 0.1 µm - 500 µm (ultra-thin freestanding films to thick cutting-tool blanks).
  • Wafer-scale diameters: Up to 125 mm for PCD equivalents; SCD available in custom orientations.
  • Surface finish: Polished to Ra < 1 nm, matching or exceeding the 8.4 nm workpiece roughness reported here—essential for mirror-edge tool fabrication.
  • Crystal orientation control: Tailored (100), (110), or (111) growth orientations to optimize wear resistance along the cutting edge.

For researchers exploring hybrid or higher-toughness alternatives, our Polycrystalline Diamond (PCD) plates (polished to Ra < 5 nm at inch-scale) provide isotropic wear behavior—useful when transitioning from prototype SCD tools to production tooling.

Customization Potential:

The 1.0 mm cutting edge width specified in this study is a critical geometry. 6CCVD offers:

  • Custom laser cutting and dicing to produce SCD/PCD tool blanks with precisely defined edge profiles and widths down to sub-millimeter tolerances.
  • Edge preparation services (chamfering, radiusing, or razor-edge lapping) to achieve the 0°/12° geometry required for ultraprecision UEVC.
  • Boron-Doped Diamond (BDD) variants for applications where electrical contact or wear-sensing is desired during cutting trials.
  • Substrate-grade diamond (up to 10 mm thick) for tool holder integration and brazing studies.

While this application does not require metallization, our in-house Ti, Pt, Au, Pd, W, and Cu metallization capabilities are available for researchers developing next-generation diamond tooling with embedded sensors, heating elements, or diffusion-bonded interfaces.

Engineering Support:

6CCVD’s in-house PhD-level engineering team routinely supports academic and industrial clients working at the intersection of diamond materials science and advanced manufacturing—including ultraprecision machining, vibration-assisted cutting, and difficult-to-cut aerospace alloys such as Inconel 718, titanium, and tungsten carbide. We can assist with:

  • Material selection between SCD, PCD, and BDD for specific wear regimes.
  • Guidance on crystal orientation, dopant levels, and surface preparation to extend tool life under thermally aggressive dry-cutting conditions.
  • Sample sizing and geometry to fit existing UEVC or diamond turning platforms (e.g., Taga EL-50Σ, Precitech Freeform, or custom Riken-class systems).

Call to Action:

For custom specifications, material consultation, or to discuss how 6CCVD’s MPCVD diamond can support your ultraprecision machining and tooling research, visit 6ccvd.com or contact our engineering team directly.

View Original Abstract

The demand for Ni-based alloys, particularly Alloy 718, is increasing in the gas turbine industry due to their high-temperature resistance and chemical stability. However, Alloy 718 is challenging to cut, owing to its susceptibility to work-harden, its high cutting resistance, and its poor thermal conductivity. Ultrasonic elliptical vibration cutting (UEVC) can be performed on steel materials using diamond tools, which is facilitated by elliptical vibration of the tool. This approach helps suppress heat generation at the tool tip and prevents chemical decomposition. In this study, we explored the precision cutting of Alloy 718 using UEVC with planar cutting and a single-crystal diamond flat tool. We achieved a surface roughness Ra of 8.4 nm at a cutting speed of 2.0 mm/s. We compared surface roughness under various conditions, including cutting speeds, the amplitude of elliptical vibration, and cutting depth, to investigate the effect of these parameters on surface roughness. Additionally, we studied the geometry and thickness of chips under these conditions using scanning electron microscopy (SEM) images. Our findings indicated flow-type chip shapes in all conditions, signifying stable ductile-regime cutting. Moreover, tool life was investigated by observing the cutting edge, which exhibited slight wear, maintaining a mirror surface for a cutting distance of approximately 50 m. These findings reveal an effective method for high-precision surface fabrication of Alloy 718, elucidating the cutting mechanism and the feasible cutting distance.