Optically stimulated luminescence characteristics of heteroepitaxial diamond with different nitrogen concentrations - effects of pre-irradiation and luminescence center activation
At a Glance
Section titled “At a Glance”| Metadata | Details |
|---|---|
| Publication Date | 2026-01-01 |
| Journal | Journal of Materials Science Materials in Electronics |
| Authors | Kiyomitsu Shinsho, Go Okada, Koji Koyama, Keitaro Hitomi, Seong Woo Kim |
| Institutions | Tokyo Metropolitan University, Kanazawa Institute of Technology |
| Analysis | Full AI Review Included |
Executive Summary
Section titled “Executive Summary”- Sapphire-based heteroepitaxial single-crystal diamond was evaluated as an optically stimulated luminescence (OSL) dosimeter at controlled nitrogen concentrations of 3 ppb and 1 ppm.
- The nitrogen-rich 1 ppm diamond produced substantially higher OSL intensity, indicating a greater density of nitrogen-related trapping and luminescent centers.
- Both materials showed weak dose dependence below 10 Gy and response saturation at approximately 100-200 Gy, consistent with depletion of available luminescence centers.
- Pre-irradiation up to 400 Gy strongly increased OSL sensitivity only in the nitrogen-rich sample, attributed to trapped-electron accumulation, activation of existing luminescent centers, and improved radiative recombination.
- The enhancement was fully reversed by annealing at 500 °C for 60 s, demonstrating a reversible occupancy effect rather than permanent defect formation.
- OSL emission was a broad 500-800 nm band peaking at 620-650 nm, characteristic of the phonon sideband associated with negatively charged nitrogen-vacancy, NV−, centers.
- The 1 ppm material also exhibited slower signal fading, indicating a higher population of thermally stable traps and potential for reusable, high-dose dosimetry.
Technical Specifications
Section titled “Technical Specifications”| Parameter | Value | Unit | Context |
|---|---|---|---|
| Diamond bandgap | 5.47 | eV | Fundamental electronic property supporting radiation hardness and deep defect states |
| Effective atomic number | ≈6 | — | Close to soft tissue, supporting tissue-equivalent dosimetry |
| Diamond growth method | MPCVD | — | Heteroepitaxial diamond layers synthesized on sapphire with an iridium buffer |
| Heteroepitaxial substrate system | Ir/sapphire | — | Sapphire-based (112̄0) misoriented substrate with an iridium buffer layer |
| Nitrogen concentration, low-nitrogen sample | 3 | ppb | HED-N_3ppb |
| Nitrogen concentration, nitrogen-rich sample | 1 | ppm | HED-N_1ppm |
| Nitrogen concentration ratio | 1000:1 | — | Difference between the two test materials |
| OSL stimulation wavelength | 850 | nm | TORAIMS optical stimulation source |
| Reference irradiation dose | 100 | Gy | Used for the reported 850 nm OSL decay-curve comparison |
| Dose range showing weak response dependence | Below 10 | Gy | Applies to both samples |
| Dose-response saturation range | 100-200 | Gy | Applies to both samples |
| Maximum reported pre-irradiation dose | 400 | Gy | Produced pronounced sensitivity enhancement only in the 1 ppm sample |
| Enhancement-reset annealing temperature | 500 | °C | Fully removed the pre-irradiation-induced sensitivity enhancement |
| Enhancement-reset annealing duration | 60 | s | Confirms reversible defect-occupancy changes |
| OSL emission range | 500-800 | nm | Broad phonon-assisted emission band |
| OSL emission peak | 620-650 | nm | Associated with the NV−-related phonon sideband |
| Resolved zero-phonon line at 637 nm | Not observed | — | Supports broad-band, phonon-assisted interpretation |
| Spectral change after pre-irradiation | None observed | — | Indicates that the same luminescent-center family remains active |
| Reported low-dose OSL behavior | Weak dose dependence | — | Potentially limits straightforward low-dose sensitivity without further optimization |
| Reported high-dose response | Saturation | — | Center-depletion model consistent with the observations |
| Fading behavior of 1 ppm material | Slower | — | Indicates a larger contribution from thermally stable traps |
| Fading behavior of 3 ppb material | Faster | — | Indicates a greater contribution from shallower or less stable traps |
| Potential application | High-dose and reusable OSL dosimetry | — | Nitrogen-rich HED is the preferred candidate |
Key Methodologies
Section titled “Key Methodologies”-
Prepare two controlled-nitrogen HED specimens
- Grow high-quality (001)-oriented heteroepitaxial diamond by microwave-plasma chemical vapor deposition.
- Use sapphire substrates with an iridium buffer layer and step-flow growth.
- Produce comparison materials with nitrogen concentrations of 3 ppb and 1 ppm.
-
Configure the OSL measurement system
- Use the TSL/OSL/RPL automated and integrated measurement system, TORAIMS.
- Stimulate the irradiated samples at 850 nm.
- Detect OSL decay using a photomultiplier or photodetection system, with an optical spectrometer available for emission-spectrum measurements.
-
Measure baseline OSL decay
- Irradiate the samples to 100 Gy.
- Record the 850 nm stimulated luminescence decay as a function of time.
- Compare the decay behavior and integrated intensity of the 3 ppb and 1 ppm samples.
-
Establish dose-response behavior
- Expose the materials across a range of irradiation doses.
- Examine OSL response from sub-gray and gray levels through the saturation range.
- Identify the low-dose region below 10 Gy and saturation at approximately 100-200 Gy.
-
Apply controlled pre-irradiation
- Pre-irradiate the nitrogen-rich sample up to 400 Gy.
- Compare OSL response before and after pre-irradiation.
- Evaluate changes in sensitivity, decay intensity, and recombination efficiency.
-
Verify the reversibility of the enhancement
- Anneal the pre-irradiated nitrogen-rich sample at 500 °C for 60 s.
- Re-measure the OSL response.
- Confirm removal of the pre-irradiation enhancement.
-
Measure the OSL emission spectrum
- Compare nitrogen-rich material before and after pre-irradiation.
- Record the broad 500-800 nm emission band.
- Determine the 620-650 nm peak and check for a resolved 637 nm zero-phonon line.
-
Assess signal fading
- Monitor OSL intensity over time after irradiation.
- Compare the 1 ppm and 3 ppb materials.
- Use the fading profiles to compare the relative stability of the involved trap populations.
6CCVD Solutions & Capabilities
Section titled “6CCVD Solutions & Capabilities”Recommended Materials
Section titled “Recommended Materials”| Research requirement | 6CCVD material recommendation | Rationale |
|---|---|---|
| Grain-boundary-free, high-crystalline-uniformity HED behavior | Optical Grade SCD | Best match for isolating impurity and point-defect effects from grain-boundary effects |
| Controlled nitrogen concentration in the ppb-to-ppm range | Custom nitrogen-engineered SCD | Nitrogen concentration should be specified and correlated with growth conditions and OSL response |
| Strong OSL intensity and thermally stable traps | Nitrogen-rich SCD, near the reported 1 ppm regime | The paper identifies the 1 ppm sample as substantially more intense and less prone to fading |
| NV−-related broad-band luminescence | Optical Grade SCD with controlled defect density | Suitable for optical dosimetry and NV-related defect spectroscopy |
| Reusable dosimeter elements | Low-roughness, optically polished SCD | Supports reproducible optical coupling, cleaning, and repeated irradiation/annealing cycles |
| Large-area or wafer-scale prototype development | PCD plates or wafers up to 125 mm | Available when device-area scalability is more important than single-crystal defect uniformity |
| High-dose detector structures with enhanced charge or defect-state control | Boron-Doped BDD or heavily boron-doped PCD | BDD is relevant when deep acceptor states and altered charge transport are required; nitrogen should not be substituted for boron without redefining the device physics |
Customization Potential
Section titled “Customization Potential”- 6CCVD can provide custom SCD and PCD dimensions, including plates and wafers up to 125 mm for PCD.
- Diamond thickness can be specified from 0.1 µm to 500 µm for SCD and PCD, with substrates up to 10 mm thick.
- SCD polishing is available to Ra < 1 nm; inch-size PCD can be polished to Ra < 5 nm.
- Custom metallization is available with Au, Pt, Pd, Ti, W, and Cu for electrode formation, conductive bonding, and detector packaging.
- Laser cutting and dimensional customization can support individual dosimeter coupons, arrays, and prototype geometries.
- For replication of the paper, the critical specification is not only nitrogen concentration but also:
- Crystal orientation and epitaxial quality
- Nitrogen incorporation uniformity
- Surface roughness
- Defect density
- Optical transmission in the 500-800 nm emission range
- Thickness and substrate configuration
- Electrode layout and optical stimulation geometry
Application-Specific Engineering Guidance
Section titled “Application-Specific Engineering Guidance”- The paper supports nitrogen-rich optical-grade SCD as the primary material for high-dose OSL dosimetry development.
- The reported saturation between 100 and 200 Gy should be considered when defining the detector operating range. For low-dose applications, additional calibration, optical geometry optimization, or alternative defect engineering may be required.
- The 500 °C, 60 s reset anneal should be treated as a process reference rather than a universal material specification. Thermal compatibility must be verified for the actual electrode stack, substrate, packaging, and intended reuse cycle.
- NV−-related emission should be confirmed through spectral measurements because the paper reports a broad phonon sideband and does not resolve the 637 nm zero-phonon line.
- Nitrogen concentration should be controlled during MPCVD growth and documented together with the growth conditions, since changes in nitrogen incorporation can alter both trap density and thermal stability.
- For detector prototypes, electrode materials and optical stimulation wavelength should be selected together. Metallization can influence thermal processing, optical collection, electrical readout, and compatibility with annealing.
Engineering Support
Section titled “Engineering Support”6CCVD’s in-house PhD team can assist with material selection and specification for similar OSL radiation-dosimetry projects, including:
- Selecting between optical-grade SCD, nitrogen-engineered SCD, PCD, and BDD
- Defining nitrogen concentration and target defect density
- Selecting SCD or PCD thickness and surface finish
- Designing electrode stacks from Au, Pt, Pd, Ti, W, and Cu
- Evaluating optical-grade polishing and low-roughness requirements
- Supporting prototype dimensions and laser-cut sample geometry
- Defining custom wafers or plates up to 125 mm
- Planning global shipment under DDU terms or DDP arrangements
Recommended Specification Path
Section titled “Recommended Specification Path”| Development stage | Recommended 6CCVD specification |
|---|---|
| Initial material screening | Optical Grade SCD, polished on both sides, thickness selected for the optical readout geometry |
| Nitrogen-response comparison | Custom nitrogen-engineered SCD at a controlled concentration, with low and elevated nitrogen comparison grades |
| High-sensitivity prototype | Nitrogen-rich SCD targeting the paper’s 1 ppm condition, subject to calibration and process validation |
| Larger-area demonstrator | PCD up to 125 mm, where grain boundaries and defect heterogeneity are acceptable for the application |
| Reusable dosimeter package | SCD element with compatible metallization and verified 500 °C, 60 s reset tolerance |
| Electrical/optical integrated device | SCD or PCD coupled with custom Au, Pt, Pd, Ti, W, or Cu electrodes and application-specific optical access |
For custom specifications or material consultation, visit 6ccvd.com or contact our engineering team directly.
View Original Abstract
This study systematically investigated the optically stimulated luminescence (OSL) characteristics of heteroepitaxial diamond (HED) with two different nitrogen concentrations (3 ppb and 1 ppm). The nitrogen-rich sample exhibited substantially higher OSL intensity than the low-nitrogen sample, reflecting an increased density of trapping sites and luminescent centers associated with nitrogen-related defects. Both samples showed weak dose dependence below 10 Gy and saturation at 100-200 Gy, consistent with the classical center-depletion model. A pronounced enhancement in OSL sensitivity was observed only in the nitrogen-rich sample following pre-irradiation up to 400 Gy. This enhancement is attributed to increased trapped-electron population, activation of previously inactive luminescent centers, and improved radiative recombination efficiency. The enhancement was completely removed by annealing at 500 °C for 60 s, indicating that the effect originates from metastable changes in defect occupancy rather than permanent defect formation. The OSL emission spectra exhibited a single broad band between 500 and 800 nm, peaking at 620-650 nm, corresponding to the phonon sideband of NV⁻-related luminescence. No zero-phonon line at 637 nm was resolved, consistent with the broad-band, phonon-assisted nature of the measured OSL emission. The spectral shape remained unchanged after pre-irradiation. Fading measurements further revealed that the nitrogen-rich diamond possesses more thermally stable trap levels than the low-nitrogen sample. These findings demonstrate that nitrogen incorporation is an effective strategy for tuning the OSL performance of HED and the potential of nitrogen-rich HED for high-dose and reusable dosimetry applications.