Analysis of Temperature Distribution During Grinding with Variable Wheel Feed
Paper details
Section titled “Paper details”| Field | Value |
|---|---|
| Journal | EAI Endorsed Transactions on Digital Transformation of Industrial Processes |
| Published | 2026-02-27 |
| Authors | Roman STRELCHUK, I. Riabenkov |
| DOI | 10.4108/dtip.11703 |
At 41.9 m/s, burnout almost never occurred during creep-feed grinding of Ti(C,N) cermet. Maximum grinding temperature stayed below 150°C across the contact arc. Burnout began near 150°C and pushed local temperature above 400°C.
Burnout threshold and contact pattern
Section titled “Burnout threshold and contact pattern”The fluid supply side had the lowest grinding temperature, below 100°C. Early peaks appeared near the center of the contact arc and moved toward the rear as material removal accumulated. Burnout then covered almost the full arc, except for the front supply region.
The paper defines θ as the increase above the pre-grinding workpiece temperature of about 25°C. It reports burnout onset at approximately 150°C and a rise above 400°C after onset. The authors predict the grinding point would reach 500°C to 600°C or more.
The cermet’s thermal conductivity was about 7 to 10 W/m·K. The authors used a Péclet-number interpretation and found workpiece heat dissipation poor. They therefore treated fluid convection as the main control on surface temperature.
The authors interpret this pattern as film boiling of the grinding fluid. Film boiling creates an insulating vapor layer that sharply reduces heat extraction. After burnout, the contact zone resembles dry grinding despite continued fluid supply.
The Jen and Lavine model agreed well with the measured waveform and reproduced the abrupt transition caused by film boiling. The paper gives no error metric for this comparison.
Direct temperature measurement
Section titled “Direct temperature measurement”The temperature was measured at the ground surface with an embedded iron-constantan Type J thermocouple. Two cermet pieces measuring 12.7 mm × 1.0 mm were joined around a 0.1 mm iron foil and a 0.076 mm constantan wire. A 0.01 mm mica sheet separated the conductors.
Grinding exposed both conductors and formed the hot junction inside the contact arc. Resistance exceeded 500 MΩ before grinding, confirming electrical isolation before the junction formed.
Calibration covered 25°C to 500°C in a temperature-controlled bath. The amplifier and linearization circuit were checked against ITS-90 iron-constantan relationships.
Smooth waveforms represented the contact temperature θ. Sharp impulses were assigned to individual abrasive grains. Only the thermocouple assembly was used during temperature trials, so force and wear tests used separate specimens.
Grinding conditions and fluid supply
Section titled “Grinding conditions and fluid supply”The abrasive was the SD270-100-HB hybrid-bonded diamond wheel. The primary wheel was 200 mm in diameter, 6 mm thick, and had a 3 mm bore. A 140 mm wheel used the same thickness and bore. The hybrid bond combined resinoid and vitrified bonding systems.
Ti(C,N) specimens were 50.8 mm or 25.4 mm long and 1.0 mm wide. The wheel depth of cut was 0.5 mm throughout. Worktable speed ranged from 40 to 80 mm/min. Tested wheel speeds were 14.7, 29.3, 41.9, and 62.9 m/s.
Coolant was a chemical-solution synthetic coolant. A high-pressure system used three precision nozzles. One nozzle entered at the fluid supply side, and two approached laterally. Table 1 reports 25 L/min, while the text reports 35 L/min. This unresolved discrepancy limits exact replication.
The wheel was trued and dressed after parameter changes. A silicon carbide cup truer ran at 134 m/min with a 100 mm/min feed and 0.02 mm depth per pass.
Worktable speed defines a burnout boundary
Section titled “Worktable speed defines a burnout boundary”Tests used a 200 mm wheel, a 14.7 m/s wheel speed, and a 0.5 mm depth of cut. After approximately 40 mm³/mm of removal, burnout appeared at worktable speeds of 60 mm/min or more. Maximum temperature then reached 400°C or above.
At worktable speeds of 50 mm/min or less, burnout never occurred regardless of the removed volume. Maximum temperature stayed below 100°C.
The results bracket a critical worktable speed between 50 and 60 mm/min under these conditions. The paper does not identify an exact critical value within that interval.
Burnout length rose rapidly with removed volume and then approached a constant value. Higher worktable speeds produced longer burnout regions. At speeds of 50 mm/min or less, effective cooling extended 3 mm to 4 mm from the supply side. That zone represented about 30% to 40% of the contact arc.
Smaller wheel diameter reduces the burnout region
Section titled “Smaller wheel diameter reduces the burnout region”Reducing wheel diameter from 200 mm to 140 mm shortened the contact arc. The absolute changes in maximum temperature and burnout length were similar for both wheels. At 14.7 m/s, the cooled section remained about 3 mm long.
At 14.7 m/s, a 0.5 mm depth of cut, and 60 mm/min table speed, burnout occurred with the 200 mm wheel. The same test avoided burnout with the 140 mm wheel. The authors therefore identify smaller wheel diameter as a way to reduce the burnout region.
Wheel speed has a thermal optimum
Section titled “Wheel speed has a thermal optimum”Figure 6 compares distributions after the grinding temperature reached steady state. The test used a 200 mm wheel, a 0.5 mm depth of cut, and an 80 mm/min table speed.
At 29.3 m/s, maximum temperature exceeded the 14.7 m/s result, and burnout began early. However, the effectively cooled section reached about 6 mm, or 60% of the contact arc.
At 41.9 m/s, burnout almost never occurred. Maximum temperature remained below 150°C along the entire contact arc. The authors propose that faster wheel motion increases fluid entrainment and shortens the time for film boiling at one location. This differs from the usual recommendation to use a low wheel speed for cermet.
At 62.9 m/s, severe burnout covered the entire contact arc. Thermal cracks formed immediately, and grinding could not continue. The authors suggest that heat generation increased while wheel airflow reduced fluid delivery. At 80 mm/min table speed, 41.9 m/s was the most stable of the tested wheel speeds.
Force and wheel wear consequences
Section titled “Force and wheel wear consequences”Normal and tangential forces were measured with a piezoelectric dynamometer mounted on the worktable. Normal force decreased as wheel speed increased. It became stable at 41.9 m/s, where burnout was almost absent.
At 14.7 and 29.3 m/s, normal force rose suddenly early in grinding. The authors attribute that rise to thermal expansion near the grinding point. Expansion increased the grain depth of cut and promoted grain fracture and pullout. Loss of active edges left the remaining grains carrying higher individual loads.
Under burnout, the authors expect reduced grain strength and reduced bond gripping strength. Higher wheel speeds produced lower radial wear rates. At lower speeds, wear against grain cutting length was nonlinear during early thermal damage. At 41.9 m/s, wear progression was more gradual and linear, consistent with attritious wear.
Earlier cited studies found less wheel wear for creep-feed than conventional pendulum grinding at constant specific material removal rate. That comparison was not repeated in this experiment. The paper reports trends but no numerical force or wear values in the extracted text.
Limits for process transfer
Section titled “Limits for process transfer”Transfer beyond this setup requires care. The tests covered one Ti(C,N) cermet, one hybrid-bonded diamond wheel, one synthetic coolant, and one three-nozzle delivery geometry. Only one wheel construction was tested, so the paper does not compare diamond grit, bond chemistry, or alternative wheel designs.
Figure 6 labels the comparison volume as 200 mm³/mm, while the text states 200 mm³/min. The paper also defines θ as a temperature rise but presents threshold values on a temperature scale.
Engineers should treat 41.9 m/s as a condition-specific operating point, not a universal wheel-speed rule. Production monitoring should track coolant delivery and the rear of the contact arc, where burnout starts.
The study does not test diamond plates, wafers, windows, membranes, or electronic devices. Any process transfer should include contact-zone temperature measurement. At 62.9 m/s, immediate thermal cracks made the grinding test impossible to continue.
View Original Abstract
INTRODUCTION: Creep-feed grinding of ultrahard cutting tool materials such as cermet presents significant thermal challenges due to extended contact arc lengths between wheel and workpiece combined with low thermal conductivity of the workpiece material. These conditions lead to dramatic temperature rises and potential burnout phenomena that compromise grinding quality and wheel life. OBJECTIVES: This study aims to experimentally investigate grinding temperature distribution within the contact arc during creep-feed grinding of cermet workpieces, identify critical burnout conditions, and determine optimal grinding parameters to enhance cooling effectiveness and prevent thermal damage. METHODS: Grinding temperature measurements were conducted using an embedded thermocouple method during creep-feed grinding of Ti(C,N) cermet alloy with hybrid-bonded diamond wheels. Temperature distributions along the contact arc were measured across various combinations of worktable speeds (40-80 mm/min), wheel speeds (14.7-62.9 m/s), and wheel diameters (140 mm and 200 mm). The onset and progression of burnout phenomena were systematically documented and analyzed. RESULTS: Experimental results revealed that burnout occurs when grinding temperature reaches approximately 150°C, causing abrupt temperature increases exceeding 400°C. Burnout initiates at the rear of the contact arc and progressively extends throughout the grinding zone. A critical worktable speed exists above which burnout occurs under constant depth of cut and wheel speed conditions. Smaller wheel diameters and optimized wheel speeds significantly improve cooling effectiveness. At wheel speed of 41.9 m/s, burnout was nearly eliminated with maximum temperatures maintained below 150°C along the entire contact arc, resulting in reduced grinding forces and wheel wear. CONCLUSION: The research demonstrates that strategic control of grinding parameters, particularly wheel speed optimization and wheel diameter selection, effectively prevents burnout and enhances cooling performance in creep-feed grinding of difficult-to-grind cermet materials. Higher wheel speeds improve grinding fluid circulation and cooling effectiveness up to an optimal threshold, beyond which excessive heat generation and reduced fluid supply negate these benefits.
Electronic Grade Intrinsic Diamond Epitaxial Wafer H Terminated Superior 100 Mosfet Ready Substrate
View Specs →
Advanced Thermal Simulation Service Diamond Heat Spreader Performance Analysis
View Specs →