Skip to content

Measuring high field gradients of cobalt nanomagnets in a spin-mechanical setup

FieldValue
JournalApplied Physics Letters
Published2026-02-02
AuthorsFelix Hahne, Teresa Klara Pfau, Liza Žaper, Lucio Stefan, Thibault Capelle
DOI10.1063/5.0301921

A cobalt nanomagnet grown by focused electron beam induced deposition produced a magnetic field gradient of 170 kT/m. The gradient was measured directly with a nitrogen-vacancy (NV) center a few hundred nanometers from the magnet. Spin coherence stayed at 20 µs or more at gradients up to 25 kT/m. The mechanical motion of the tuning fork modulated the spin decay. The authors place this combination in hybrid platforms that use a high-Q resonator in a magnet-on-oscillator configuration.

Spin-mechanical platform and how the gradient is measured

Section titled “Spin-mechanical platform and how the gradient is measured”

The experiment uses a scanning NV microscopy configuration with x, y, z piezo nanopositioners that place the tuning fork relative to the nanomagnets with nanometer resolution. The core of the setup is a 100-cut diamond scanning probe hosting the NV center on a quartz tuning fork. The probe faces a silicon chip carrying the cobalt nanomagnets and an integrated microwave stripline for spin control. The nanomagnet studied here sits about 40 µm from the stripline and has a cylindrical shape with 830 nm height and 400 nm diameter.

Bias fields up to 140 mT come from a 4 cm diameter spherical NdFeB permanent magnet with a residual field density of 1.26 to 1.29 T. The magnet is aligned to the NV quantization axis. Excitation uses 515 nm laser light through a 0.9 NA objective on a home-built confocal microscope. The stray field is read from the Zeeman shift of the lower energy ODMR resonance. The ground state zero field splitting is ν0 ≈ 2.87 GHz and the gyromagnetic ratio is γNV ≈ 28 GHz/T. The NV center lies 70 ± 20 nm below the probe apex, a depth obtained by comparing probe topography with a commercial AFM.

Focused electron beam deposition of the cobalt nanomagnet

Section titled “Focused electron beam deposition of the cobalt nanomagnet”

The cobalt structures are grown by FEBID from Co2(CO)8 precursor released through a gas injection system into the vacuum chamber. On the silicon chip the electron beam follows a circular raster pattern from the center outward. Growth parameters are an acceleration voltage of 5 kV, a beam current of 100 pA, and a dwell time of 1 µs. The precursor flux corresponds to a vacuum pressure of 1.1 × 10⁻⁶ to 1.2 × 10⁻⁶ mbar.

Deposited structures show a systematic offset from the defined diameter, between 20 nm and 100 nm. The offset comes from charging, the so-called halo, produced by secondary electrons scattering off the substrate and the grown deposit. In a circular pattern the irradiation time per area is highest at the center, which raises charging there, while a raster-scanned rectangular pattern is more uniform.

On thin insulating SiN membranes, which charge strongly under the electron beam, the authors switched to a rectangular beam pattern. That pattern produced circular structures with 100 nm diameter on membranes 50 nm thick. The membrane growth used a precursor flux corresponding to a pressure of 1.72 to 2.78 × 10⁻⁶ mbar. Nanomagnets are placed 30 µm to 210 µm from the stripline and separated laterally by 60 µm, enough to prevent mutual stray field interaction.

The stripline is fabricated on 4-inch high-resistivity silicon wafers above 20000 Ω cm, polished on one side and 500 ± 25 µm thick, with a 5 nm chromium adhesion layer and 100 nm gold. Chips are diced with a diamond saw, cleaned, and wirebonded to a printed circuit board that provides the microwave contacts.

Magnetometry was done by raster scanning xy planes above a single nanomagnet under ambient conditions, without feedback, at a fixed height above the substrate. Four maps were acquired at heights from 960 nm to 1460 nm above the nanomagnet, in steps of 166 ± 5 nm. A simultaneous dipole fit across all four maps fixed the relative height offsets and constrained the dipole depth and moment. All scanned maps showed stray field patterns consistent with a magnetic dipole field.

The fitted dipole moment magnitude grows linearly with the external bias field between 30 mT and 140 mT. The authors attribute this to the soft magnetic nature of the typically amorphous FEBID structure. A simulation built on the dipole fit and AFM topography reproduces the same moment curve. The net magnetic moment obtained by volume integration of the simulated magnetization agrees with both the measured and fitted values. The authors read this agreement as mutual validation across measurement, model, and simulation.

Micromagnetic simulation and saturation behavior

Section titled “Micromagnetic simulation and saturation behavior”

The simulation uses MuMax3 with an exchange stiffness of 14 × 10⁻¹² J/m and zero magnetocrystalline anisotropy. The saturation magnetization is set to 1.26 MA/m, which is 90% of the bulk value for non-annealed structures. The voxel size is 36.83, 30, and 25 nm on a grid of 120 × 100 × 110 cells, built from AFM topography.

The simulation predicts that the nanomagnet approaches saturation at a bias field of about 300 mT. The measured ratio 140 mT / 300 mT = 0.47 matches the magnetization ratio M/Msat = 0.45 obtained from the measured moment and the nanomagnet volume.

Spin decay was measured with a spin echo sequence, with π pulse durations of about 55 ns calibrated by Rabi measurements at each position. Visibility is computed from two echo measurements whose final readout pulse is applied along the +X or -X axis, which rejects common-mode noise. At a gradient of 4.4 ± 1.6 kT/m the extracted spin echo time is 34.0 ± 5.3 µs. Away from the nanomagnet the same measurement returns 56 ± 6 µs. Measurements were taken at distances of about 540 nm to 1587 nm from the nanomagnet.

The coherence time falls as the gradient grows. The authors attribute this to magnetic noise from the nanostructure, or to thermal drifts that fluctuate the NV center frequency and cause dephasing. Coherence of at least 20 µs was preserved up to 25 kT/m.

A microwave drive near the NV and the nanomagnet heats the assembly and shifts the ODMR resonance. Accurate on-resonance pulses therefore cannot be applied above 30 kT/m. Horizontal error bars come from measuring the gradient before and after each echo sequence.

Tuning fork motion modulates the spin signal

Section titled “Tuning fork motion modulates the spin signal”

The tuning fork is driven at its resonance frequency and vibrates along the x direction, where the NV center sits in a gradient Gx ≈ 540 T/m. Without drive the echo visibility decays undisturbed with a time of 42 ± 3 µs. With drive at Ωm ≈ 32 kHz, the decay becomes modulated. The modulated curves fit a zeroth-order Bessel function, which the authors read as evidence of spin-mechanical coupling.

The fit returns a motion amplitude of 3 ± 1 nm at a piezo drive amplitude of 3 mV. At 9 mV drive the amplitude is 11 ± 1 nm. The mechanical motion maps into an oscillating magnetic field of 2.0 ± 0.6 µT and 6.1 ± 0.8 µT at the NV center.

Projected coupling to a high-Q resonator and open questions

Section titled “Projected coupling to a high-Q resonator and open questions”

The authors estimate the coupling for a future device with a 1.5 MHz resonance, an effective mass of 2 ng, and a quality factor of 10⁹ at 4 K. Combining a spin coherence time of 1 ms with the measured 170 kT/m gradient gives a single-phonon coupling strength g0/2π = 8 Hz. The corresponding cooperativity is 5 × 10⁻³, four orders of magnitude above current state-of-the-art setups. The thermal force noise of that resonator would be 4 aN²/Hz. The force produced by the oscillating spin, F = µB G = 1.6 aN, is of similar size. The authors conclude that the spin force could be detected within a few seconds of averaging, during which the spin is re-polarized.

Reaching cooperativity near one is harder. It would require a spin coherence time of 10 ms and a gradient of 1 MT/m, predicted to be reachable at 150 nm from the magnetic structure at saturation.

Several limits are visible in the data. Approaching the surface closer than about 250 nm drops the ODMR signal-to-noise ratio below unity, which the authors attribute to mechanical drift from microwave heating. The measurement assumes a dipole field, neglects local off-axis strain, and takes the bias field as aligned with the spin axis. The effect of the deposition on the mechanical quality factor of a membrane is still open. The authors list it as a necessary step before quantum spin-mechanics applications. Operating at cryogenic temperatures with active stabilization could allow spin manipulation at higher gradients, the authors expect.

The platform runs on a diamond scanning probe hosting a single NV center 70 ± 20 nm below the apex. 6CCVD grows single-crystal diamond by MPCVD, with plates up to 125 mm, thickness from 0.1 µm, polishing to Ra below 1 nm, and Au metallization. Those plates and metallization options are in the diamond materials catalog, and probe shaping can be taken up on the engineering support page.

View Original Abstract

Hybrid systems composed of a single nitrogen-vacancy center spin magnetically coupled to a macroscopic mechanical resonator constitute promising platforms for the realization of quantum information protocols and for quantum sensing applications. The magnetic structure that mediates the interaction must ensure high field gradients while preserving the spin and mechanical properties. We present a spin-mechanical setup built around a cobalt nanomagnet grown with focused electron beam-induced deposition. The magnetic structure is fully characterized, and a maximum gradient of 170 kT m-1 is directly measured at a spin-oscillator distance of a few hundred nanometers. Spin coherence was preserved at the value of 20μs up to a gradient of 25 kT m-1. The effect of the mechanical motion on the spin dynamics was observed, thus signifying the presence of spin-mechanics coupling. Given the noninvasive nature of the nanomagnet deposition process, we foresee the adoption of such structures in hybrid platforms with high-quality factor resonators, in the “magnet on oscillator” configuration.