Optically detected magnetic resonance of nitrogen-vacancy centers in microdiamonds inside nanopolycrystalline diamond anvil cell
Paper details
Section titled “Paper details”| Field | Value |
|---|---|
| Journal | Japanese Journal of Applied Physics |
| Published | 2026-03-09 |
| Authors | Masahiro Ohkuma, Keigo Arai, Kenji Ohta, Toru Shinmei, Ryo Matsumoto |
| DOI | 10.35848/1347-4065/ae4f44 |
Continuous-wave optically detected magnetic resonance was detected from nitrogen-vacancy centers in microdiamonds inside a nanopolycrystalline diamond anvil cell at inferred pressures above 30 GPa. The cell used 600 µm culets. A five-microdiamond wide-field measurement produced resonances from 3.28 GHz to 3.39 GHz. These frequencies correspond to inferred pressures of 28 GPa to 35 GPa.
Nanopolycrystalline diamond as the anvil
Section titled “Nanopolycrystalline diamond as the anvil”Nanopolycrystalline diamond (NPD) supports optical access while limiting heat loss from the sample chamber. NPD contains fine grains several tens of nanometers in random crystallographic orientations. Its optical transparency is comparable to typical Type Ib single-crystal diamond (SCD). The absence of cleavage planes gives NPD superior hardness and isotropic mechanical properties.
Its thermal conductivity can be nearly an order of magnitude below typical SCD. Laser-heated NPD cells have reached temperatures exceeding 5000 K. That thermal behavior is a cited NPD capability, not a temperature reached in this experiment.
These properties suit spectroscopy and large-volume high-pressure work. However, grain boundaries, defects, and dislocations may scatter light and emit background luminescence. The NPD photoluminescence was 4% of the microdiamond signal in this setup. The Type IIa SCD background was below the APD detection limit. The authors warn that weaker emitters could reduce the signal-to-background ratio.
Cell construction and microwave coupling
Section titled “Cell construction and microwave coupling”Two opposing NPD anvils had 600 µm culets. A rhenium gasket started at 250 µm and was pre-indented to 50 to 60 µm. A 200 µm hole formed the sample chamber, and glycerol served as the liquid pressure-transmitting medium.
Several 15 to 25 µm microdiamonds with 3.5 ppm NV centers sat on the culet surface before sealing. For focused measurements, cBN and TiO2 protected the slit and Lenz lens before the sample space was filled. Some cBN and TiO2 contamination remained during sealing.
A 1.5-turn copper loop around the anvil supplied the microwave magnetic field for focused measurements. Wide-field measurements used a platinum foil on the culet as a microwave antenna. The foil had no electrical insulation layer.
| Measurement mode | Gasket hole | Microwave coupler | Detector |
|---|---|---|---|
| Focused APD | 200 µm | 1.5-turn copper loop | Avalanche photodiode |
| Wide-field EMCCD | 300 µm | Platinum foil antenna | EMCCD camera |
The wide-field gasket omitted the Lenz lens.
ODMR setup and pressure calibration
Section titled “ODMR setup and pressure calibration”Each negatively charged NV center has spin (S=1), with a 2.87 GHz zero-field resonance at ambient conditions. Its ground-state splitting responds to temperature, magnetic field, and pressure.
Continuous-wave ODMR used a 532 nm laser and a 20x objective. Red fluorescence passed through a long-pass filter before reaching an APD or EMCCD. All ODMR measurements were made at room temperature. Each APD and EMCCD spectrum required no more than 10 minutes.
Pressure was inferred from the fitted resonance frequency using (P_{\mathrm{ODMR}}=(D-D_0)/\beta), with (D_0=2.87) GHz and (\beta=14.58) MHz/GPa. Here, (D) was the fitted resonance frequency. The error bars in Figure 3 represent 95% confidence intervals for fitted (D).
Two resonance dips were visible at ambient pressure. The authors attribute their splitting to local strain or local electric fields from charged defects or impurities. Pressure shifted both resonances toward higher frequencies and reduced photoluminescence.
The contrast was approximately 8% at 20 GPa. The authors say this contrast could permit ODMR at higher temperatures, where signal and contrast decrease. They did not measure elevated-temperature ODMR in this study.
Pressure cycling and signal recovery
Section titled “Pressure cycling and signal recovery”ODMR spectra were recorded during compression from ambient pressure and during decompression back to ambient pressure. Photoluminescence recovered as pressure decreased. The P10 signal remained approximately 50% of the pre-compression signal after full pressure release.
The authors propose that microdiamond movement and residual cBN and TiO2 blocked part of the fluorescence. The splitting changed during decompression. It was larger at P9 than at P7 and P8.
The authors suggest that P7 and P8 contained a broader strain distribution, while contact redistribution made narrower environments dominant at P9. They also note that relaxation changes and inhomogeneous broadening remain unresolved. A quantitative separation of these effects requires established zero-field lineshape analysis.
Local pressure and magnetic response
Section titled “Local pressure and magnetic response”At pressure sequence P6, the authors measured three microdiamonds with separate resonances.
| Microdiamond | Resonance frequency | Inferred pressure | Condition |
|---|---|---|---|
| NV1 | 3.175 ± 0.005 GHz | 20.9 ± 0.3 GPa | P6, room temperature |
| NV2 | 3.127 ± 0.004 GHz | 17.6 ± 0.3 GPa | P6, room temperature |
| NV3 | 3.130 ± 0.002 GHz | 17.8 ± 0.1 GPa | P6, room temperature |
These estimates describe local effective pressures rather than a single chamber pressure. The paper cites ruby measurements with a standard deviation of about 2 GPa near 20 GPa for a methanol, ethanol, and water medium. The authors recommend simultaneous ruby fluorescence as an independent check of the ODMR pressure scale and distribution.
At P8, a permanent magnet produced clear field-dependent changes in the NV1 spectrum. This establishes a magnetic response in the NPD geometry, but the paper does not report a calibrated magnetic-field value.
Wide-field readout and pressure spread
Section titled “Wide-field readout and pressure spread”Wide-field ODMR captured five microdiamonds, NV4 through NV8, in one EMCCD image. Their resonance frequencies ranged from 3.28 GHz to 3.39 GHz. The corresponding inferred pressures ranged from 28 GPa to 35 GPa. Pressures from different microdiamonds differed by more than 10%.
The authors relate this spread to pressure inhomogeneity and deviatoric stress after the transmitting medium solidifies. Each microdiamond therefore samples its own local environment.
Previous work reported pressures up to approximately 80 GPa with millimeter-class NPD culets. Cited studies have operated NV centers at pressures up to 100 GPa. This work demonstrates an NPD geometry rather than the highest pressure reached by an NV sensor.
Limits for temperature and quantitative imaging
Section titled “Limits for temperature and quantitative imaging”All measurements in this study were at room temperature, so concurrent high-pressure and high-temperature operation was not demonstrated. ODMR contrast decreases at elevated temperature and under non-hydrostatic stress. Broadening and splitting can hinder quantitative analysis.
Random microdiamond orientations produce overlapping resonances from several NV axes under a bias field. The authors suggest hydrostatic gas loading, a defined-orientation sensor chip, or both for quantitative magnetic imaging.
NV formation and stability within NPD remain uncertain at room temperature. A 637 nm photoluminescence peak was observed in as-grown NPD at 5 K. The material contained approximately 100 ppm nitrogen, while its P1 center concentration was below 1 ppm. Future work could examine NV implantation or chemical vapor deposition in NPD.
Earlier cited studies operated NV spin control at 1400 K. Those operating records do not apply to the NPD cell tested here. The authors propose integrating NV microdiamonds with boron-doped diamond electrodes, heaters, and a microwave circuit. The paper cites boron-doped diamond deposition on NPD by microwave plasma chemical vapor deposition. This integration was proposed, not demonstrated in the reported ODMR experiment. The authors state that a boron-doped diamond electrode can be reused until the diamond breaks.
Materials and support
Section titled “Materials and support”The high-pressure sensor requires NV-containing microdiamonds and nanopolycrystalline diamond anvils, with Pt and Cu used in its microwave coupling. 6CCVD’s diamond materials catalog lists boron-doped diamond and metallization with Pt and Cu, which are relevant to the paper’s proposed electrodes, heaters, and microwave circuitry. The engineering support link can discuss custom component requirements, although the catalog does not list NV-containing microdiamonds.
View Original Abstract
Abstract We demonstrated optically detected magnetic resonance (ODMR) of nitrogen-vacancy (NV) centers in microdiamonds inside a diamond anvil cell pressurized with nanopolycrystalline diamond (NPD) anvils. NPD exhibits high optical transparency, superior hardness, and low thermal conductivity, making it suitable for optical and spectroscopic measurements under high-pressure and high-temperature conditions. We observed the ODMR signal from an ensemble of NV centers under conditions where NV centers in microdiamonds served as markers for pressures exceeding 30 GPa, with a culet diameter of 600 μ m. We also performed ODMR measurements on multiple microdiamonds sealed inside a sample chamber and found that the resonance frequency varied with the pressure distribution. The combination of NPD and microdiamonds containing NV centers is auspicious for pressure and magnetic sensing under concurrent high-pressure and high-temperature conditions.
Boron Doped Single Crystal Diamond Plate
View Specs →
Boron Doped Diamond On Titanium Bdd Electrode
View Specs →
Boron Doped Diamond Electrode On Niobium Bdd Nb Electrode
View Specs →References we cover
Section titled “References we cover”- GPa Pressure Imaging Using Nanodiamond Quantum Sensors
- Imaging magnetic transition of magnetite to megabar pressures using quantum sensors in diamond anvil cell
- Wide-field magnetometry using nitrogen-vacancy color centers with randomly oriented micro-diamonds
- High-Pressure Synthesis of Superconducting Sn3S4 Using a Diamond Anvil Cell with a Boron-Doped Diamond Heater
- AC sensing using nitrogen vacancy centers in a diamond anvil cell up ton 6 GPa
Original source
Section titled “Original source”References
Section titled “References”- 2019 - Imaging stress and magnetism at high pressures using a nanoscale quantum sensor [Crossref]
- 2019 - Magnetic measurements on micrometer-sized samples under high pressure using designed NV centers [Crossref]
- 2019 - Measuring magnetic field texture in correlated electron systems under extreme conditions [Crossref]
- 2021 - Recent developments of quantum sensing under pressurized environment using the nitrogen vacancy (NV) center in diamond [Crossref]
- 2024 - Imaging the Meissner effect in hydride superconductors using quantum sensors [Crossref]
- 1988 - Optically detected spin coherence of the diamond N-V centre in its triplet ground state [Crossref]
- 1997 - Scanning confocal optical microscopy and magnetic resonance on single defect centers [Crossref]
- 2004 - Observation of coherent oscillations in a single electron spin [Crossref]
- 2013 - The nitrogen-vacancy colour centre in diamond [Crossref]
- 2010 - Temperature dependence of the nitrogen-vacancy magnetic resonance in diamond [Crossref]