Plastic deformation in nanodiamonds
Paper details
Section titled “Paper details”| Field | Value |
|---|---|
| Journal | Nature Communications |
| Published | 2026-03-05 |
| Authors | Jiaqi Zhang, Chunmeng Liu, Xing Li, Lilin Xie, Y.F. Zhang |
| DOI | 10.1038/s41467-026-70189-6 |
| Citations | 2 |
Nanodiamonds below about 13 nm sustained compressive strains exceeding 90% without fracture at room temperature. The four-cycle test used a particle with an initial diameter of 7.3 nm. Compressed particles reached about 0.4 nm thickness, close to the theoretical near-single-atomic-layer limit. The authors attribute this behavior to subnanometer amorphous carbon networks that permit grain sliding and rotation. This differs from dislocation-controlled plasticity reported for larger diamond.
A sharp size boundary controls the deformation mode
Section titled “A sharp size boundary controls the deformation mode”Particles smaller than about 13.2 nm consistently formed a stable sp²/sp³ amorphous network and sustained ultralarge plastic deformation. Particles from 17 to 100 nm cracked and split without forming a continuous amorphous phase. The authors place the crossover between about 13 and 15 nm. They propose that a continuous subnanometer network becomes energetically unfavorable above that range.
Both single-crystalline and polycrystalline particles showed the small-size response. Compression along different crystallographic orientations also produced the same mechanism. This result places plasticity in a confined nanoscale regime rather than treating it as a general diamond property. At submicrometer scales, earlier diamond studies attributed plasticity mainly to dislocation generation and motion. The paper argues that nanoscale diamond uses a different carrier for permanent strain.
In situ TEM captures deformation and forces
Section titled “In situ TEM captures deformation and forces”Explosion-made particles with sub-10 nm diameters were cleaned in aqua regia for at least 24 hours. Most experimental particles were single-crystalline, and polycrystalline particles served as comparison samples.
Diamond indenters attached to tungsten wires compressed one particle inside a custom TEM holder. One indenter was driven by a piezoelectric actuator toward a fixed indenter. The instrument used a length extensional resonator operating near 1 MHz. Its oscillation amplitude was about 20 pm, so displacement transmitted to the particle stayed below the 154 pm C-C bond length.
Stiffness came from the resonant frequency shift, while force came from integrating stiffness over compression distance. Stress used the effective particle diameter and the method of Stauffer and colleagues. Plasticity was identified from resonator energy dissipation, which rose above zero during irreversible deformation. Measurements ran at room temperature, about 300 K, under 10⁻⁷ Pa vacuum.
The authors repeated compression at 200 kV and 80 kV under beam blanking. Identical behavior indicated mechanical loading, not radiolysis or knock-on damage, caused the transformation. Disabling resonant oscillation also reproduced the behavior, ruling out high-cycle fatigue. Feedback fluctuations and signal noise did not change the overall trends.
Plasticity proceeds through distinct structural stages
Section titled “Plasticity proceeds through distinct structural stages”The initial response was elastic, with a maximum elastic strain of about 12%. At approximately 14% strain, dissipated energy rose to about 0.09 eV per cycle. The particle flattened and expanded laterally without cracks or abrupt displacement. Estimated stress at this stage was about 58 GPa.
During the next cycle, amorphous regions appeared and expanded around 45% strain. Nanobeam diffraction and EELS confirmed the loss of long-range crystalline order. Those amorphous regions contained both sp² and sp³ bonding. Continued loading divided the particle into 2 to 5 nm grains. The grains rotated by an estimated 10 to 20 degrees and slid along the amorphous layers. No dislocation arrays or shear bands explained the reorientation.
By a strain above 60%, the particle was almost entirely amorphous. It eventually reached about 0.4 nm thickness without nanocracks, voids, or discontinuities.
| Regime | Structural observation | Mechanical response |
|---|---|---|
| Early plastic flow | The particle flattened without cracks at about 14% strain. | Dissipation reached about 0.09 eV per cycle, with stress near 58 GPa. |
| Amorphization | Mixed sp²/sp³ regions expanded and divided the particle. | Dissipation was about 0.09 eV per cycle before falling to about 0.05 eV per cycle. |
| Grain rearrangement | Grains of 2 to 5 nm slid and rotated by about 10 to 20 degrees. | Dissipation stayed near 0.05 eV per cycle. |
| Final mixed stage | Some grains amorphized while others continued to move. | Dissipation changed from about 0.05 to 0.06 eV per cycle. The particle was almost fully amorphous above 60% strain. |
The authors interpret the higher dissipation as greater energy demand for breaking ordered sp³ bonds. The lower dissipation during rearrangement supports this distinction. Stiffness also fell during the later stage. The authors therefore separate bond-breaking amorphization from grain motion. Repeated particles showed smooth structural evolution without sudden stiffness drops.
Bonding changes identify the stress-accommodating network
Section titled “Bonding changes identify the stress-accommodating network”Progressive EELS mapping tracked sp² bond formation as strain increased. The measured sp² fraction rose from about 15% at 16% strain to about 30% at 45% strain. It then saturated around 35 to 40% at about 72% strain. The π* peak grew gradually, while the σ* signal represented the retained sp³ population.
Mapping showed sp² regions nucleating first at stressed particle ends. These regions connected into a continuous subnanometer mixed network between reoriented grains. The authors describe this network as the structure that carries large plastic strain. It also binds fractured nanograins, allowing cooperative rotation and translation. Amorphous layers measured less than 1 nm in the reported images.
Such layers have negligible mechanical influence in bulk diamond, but they become relevant when grains are only a few nanometers. Unlike a shear band, the network redistributes stress at atomic scale without serving only as fracture initiation.
Molecular dynamics reproduces the observed sequence
Section titled “Molecular dynamics reproduces the observed sequence”An 8 nm single-crystal particle was modeled with the Tersoff force field at 300 K. Simulation used a 1 fs timestep and an indenter speed of 0.01 nm per ps. Local amorphous regions first appeared inside or on the particle surface. They multiplied, merged, and partitioned the particle into small crystalline grains. The grains then moved relative to one another before complete amorphization.
The simulated elastic-to-plastic transition occurred near 55 GPa, close to the measured 58 GPa. Stress rose while amorphous regions propagated and fell when grain sliding began. Simulations generated only a limited number of dislocations, supporting amorphization as the main plasticity carrier. Runs along [100], [110], and [111] produced interconnected amorphous layers. Simulated structures also approached a single-atomic-layer thickness under extreme compression.
The uncompressed particle showed seven crystalline neighbor peaks, while the compressed particle resembled amorphous carbon. Local amorphous and crystalline domains coexisted over a wide strain range. The authors contrast this sustained flow with ceramic plasticity, which they report as typically below 10% and often preceding fracture. Earlier diamond pillar and film studies associated deformation with dislocation glide or twinning rather than a connected amorphous network.
Compression can fuse nanodiamond particles
Section titled “Compression can fuse nanodiamond particles”Two adjacent particles merged into one particle under compression without melting or external heating. Head-to-head compression also produced direct fusion. Repeated compression fused several particles into a larger particle that retained ultralarge plasticity. High-resolution TEM showed a continuous interface without visible voids or separation. The merged particles shared an amorphous network that reorganized into a nanograined structure. This created mechanical bonding rather than a crack boundary.
The authors present cold welding as a nanoscale assembly and processing method. Applications they propose include nanoelectromechanical systems, quantum information processors, and next-generation nanoelectronic devices. These are proposed uses, not demonstrated device performance.
What the result does and does not establish
Section titled “What the result does and does not establish”The final atomic arrangement was not resolved directly at the 0.4 nm compressed thickness. Near-single-layer contrast in high-resolution images most likely represents an ultrathin amorphous layer below 1 nm. The authors infer the upper size boundary from observed behavior and an energetic argument. The experiments compressed individual particles at room temperature, so tensile plasticity and temperature dependence were not tested. The work therefore supports plastic compaction, grain rearrangement, and fusion for particles below the reported size range.
For material selection, the 13 to 15 nm boundary is more relevant than a generic claim of diamond ductility. Device design must control particle size and verify whether amorphization changes the intended electronic or optical function. The paper associates controlled amorphization with possible mechanical or functional benefits, but it does not test those functions. Mechanical fusion at the nanoscale was demonstrated, rather than a bulk joining process.
The supplied manuscript is an unedited article-in-press version, so final wording and figures may change.
Materials and support
Section titled “Materials and support”The paper uses nanodiamond from below about 13 nm to 100 nm, including single-crystalline and polycrystalline particles, for deformation and cold-welding experiments. 6CCVD’s diamond materials catalog includes single-crystal and polycrystalline MPCVD-grown diamond, which covers the study’s crystallinity classes but not its explosion-made preparation or particle-size range. The engineering support page can clarify whether a related experiment can use a supplied particle geometry and size.
View Original Abstract
Diamond, composed of sp³ covalent carbon bonds, is renowned for its exceptional hardness, thermal conductivity, and wide bandgap, yet its intrinsic brittleness severely limits deformation and processing. Here, we report an amorphization-mediated ultralarge plasticity in nanodiamonds using a custom-designed in-situ transmission electron microscopy mechanical holder. Unlike conventional mechanisms such as dislocation motion or crystalline phase transformation, the deformation is governed by the formation of an interconnected amorphous carbon network that accommodates stress and enables cooperative grain rotation and sliding. This amorphization-mediated plasticity allows nanodiamonds to sustain compressive strains exceeding 90% without fracture. A distinct size-dependent transition is identified: ultralarge plasticity occurs only below ~13 nm, while larger diamonds deform in a brittle manner. This work provides critical insights into nanoscale mechanics and offering exciting opportunities for diamond-based nano-manufacturing, strain engineering, and advanced quantum or electronic device applications. Nanodiamonds below ~13 nm deform plastically by forming ultrathin amorphous carbon networks, enabling over 90% compression without cracking. In situ TEM and simulations reveal this mechanism, opening routes for nanoscale diamond shaping and assembly.
High Concentration Quantum Grade Single Crystal Diamond
View Specs →Products