High-sensitivity optical detection of electron-nuclear spin clusters in diamond
Paper details
Section titled “Paper details”| Field | Value |
|---|---|
| Journal | Physical Review Research |
| Published | 2026-04-25 |
| Authors | L. Chambard, A. Durand, J. Voisin, M. Perdriat, V. Jacques |
| DOI | 10.1103/g88t-fddb |
Room-temperature optical detection resolved four 13C nuclear-spin families and eight coupled-pair transitions around negatively charged NV centers. The main measurements used a magnetic field of 486.8 G. The authors measured all three hyperfine-tensor components for each family and obtained a 13C nuclear coherence time of 203(9) µs. The work demonstrates ensemble NMR readout through NV photoluminescence under modest fields. Earlier high-resolution 13C studies mainly used probabilistic measurements of several single NV centers, while bulk ensemble measurements often relied on conventional NMR with Tesla-scale fields and cryogenic temperatures.
Experimental configuration
Section titled “Experimental configuration”The measurements used a homemade confocal microscope. Green lasers delivered 200 mW to excite the NV centers. Balanced photoluminescence detection and active correction of beam pointing and amplitude noise reduced laser noise during wideband scans.
The sample was Element Six BNV14, a CVD-grown diamond containing 4.5 ppm NV centers and 1.1% natural-abundance 13C. The optical spot covered about 5 µm² at the surface and produced up to 40 µW of stable photoluminescence. Referenced to the green laser, the noise remained near 10^-4 V for more than an hour.
A pair of 2-inch permanent magnets generated the field. Most measurements used 486.8 G aligned with one of four NV center families. This is near the excited-state level anticrossing around 500 G, where the transverse excited-state hyperfine interaction enables nuclear-spin polarization. Polarization used relative angles below 1 degree between the magnetic and NV axes.
ODMR and ODNMR near the anticrossing
Section titled “ODMR and ODNMR near the anticrossing”Continuous green illumination and an RF tone provided optically detected nuclear magnetic resonance. An RF-driven nuclear flip produced an electron-nuclear flip-flop in the excited state. The electron then entered the minus-one electronic state and decayed nonradiatively through the metastable state, lowering photoluminescence.
At 487 G, the principal ODMR line was 1506 MHz with a linewidth of about 0.9 MHz. Its linewidth was close to the value at approximately 50 G, indicating negligible field inhomogeneity. Earlier observations of proximal family A had about 2 MHz resolution.
An electron spin echo sequence gave 521(5) kHz oscillations at 487(1) G, matching 13C Larmor precession. The echo envelope decayed with T2 of about 7(3) µs, while T2* was about 1 µs. Direct ODMR hyperfine extraction was limited by 1/T2*. ESEEM resolution was limited by 1/T2, or about 140 kHz. Equivalent sites within one family broadened the Fourier peaks.
Nitrogen spin detection in two charge states
Section titled “Nitrogen spin detection in two charge states”At 10 mW continuous-wave optical power, all four 14N nuclear transitions in the minus-one and plus-one electron manifolds were visible without microwave pulses. Lower optical power prevented full electronic polarization, allowing nuclear transitions to affect photoluminescence directly.
Readout at the anticrossing favored the minus-one electronic manifold. This raised contrast for one 14N transition and lowered contrast for another, even though the latter nuclear state was better polarized.
In the neutral NV state, resonances appeared at 1.472(9), 1.782(3), 7.540(8), and 7.828(3) MHz. The analysis gave a quadrupole magnitude of 4.655(5) MHz, a longitudinal hyperfine term of 6.057(3) MHz, and a perpendicular term of 3.9(6) MHz. The perpendicular component had not been reported before, to the authors’ knowledge.
The readout protocol first polarized 14N in the negatively charged state. A two-photon process converted the center to the neutral state, RF drove the nuclear spin, and a second photoionization returned the center to the negative state. The transition contrasts were consistent with substantial nuclear polarization surviving conversion. The neutral state lacks spin-selective optical transitions, which restricts coherent spin control.
Identifying 13C families and measuring hyperfine tensors
Section titled “Identifying 13C families and measuring hyperfine tensors”Sharp resonances in the minus-one and plus-one electronic states identified the A, B, C, and D 13C families. At 486.8 G, the four peaks in the zero-projection state were 469.79(3), 480.27(5), 499.29(9), and 516.58(5) kHz.
The authors did not assign these peaks by order because the perpendicular hyperfine ordering can differ from the longitudinal ordering. They used two-tone correlation spectroscopy to make the assignment. A modulated RF pump addressed one zero-projection peak while a second RF tone scanned a transition in the minus-one state. The lock-in signal appeared only when both tones addressed the same family. No cross-signals appeared among the 16 measurements. Thus, the peaks were assigned to families A, B, C, and D in ascending frequency.
To lowest order, each zero-projection peak position determines the absolute perpendicular hyperfine term independently of the longitudinal term. An off-axis field up to 0.085 mT split the A and B transitions and lifted the site degeneracy within those families. A two-dimensional scan covered transverse fields from -0.15 mT to 0.15 mT. Fitting the split curves produced the anisotropic hyperfine term.
| 13C family | Sites | (A_\perp) (MHz) | (A_{\rm ani}) (MHz) | (A_\parallel) (MHz) |
|---|---|---|---|---|
| A | 6 | 15.6(1) | 1.56(8) | 13.7496(1) |
| B | 3 | 14.00(7) | 1.8(1) | 12.795(2) |
| C | 3 | -10.4(1) | 0.9(2) | -8.9(2) |
| D | 6 | -5.2(2) | 0.90 | -6.51(2) |
The transverse sign was set to match the longitudinal sign. The measured terms showed good agreement with the prior hyperfine calculation.
Coherent control and coupled spin pairs
Section titled “Coherent control and coupled spin pairs”A Ramsey sequence on 14N used an RF tone detuned by approximately 8 kHz from the central transition at 5.091 MHz. The fit gave a T2* of 864(7) µs. This was close to the NV electronic spin T1 and the estimate derived from the electronic T2*.
A 13C Ramsey measurement fixed the RF at 460 kHz. The fit gave components at 9.87(3) and 20.34(6) kHz, plus a feature near 40 kHz from family C. The fitted 13C coherence time was 203(9) µs. The authors interpret the comparable ratios of coherence times and gyromagnetic ratios as evidence for a common decoherence origin in the two nuclear species.
The NV electronic spin also mediated coupling between two nearby 13C nuclei. The transition from the ground state to the triplet state was allowed, while the singlet-state transition was forbidden. The calculated ratio of double occupancy to single occupancy was 1/10, which made pair detection feasible in about an hour with the setup.
Eight of the nine listed pair transitions were observed. For example, the A-A transition was 360.1(3) kHz compared with a predicted 359.2(1) kHz. The B-D transition was 462.1(7) kHz compared with 460.4(1) kHz. The D-D transition had a predicted frequency of 504.7(1) kHz but no reported experimental value.
Current limits and engineering implications
Section titled “Current limits and engineering implications”The ensemble ODMR method inherits the electron spin coherence limit of about 1 µs. ESEEM offers finer frequency resolution, but inequivalent sites within each 13C family broaden its peaks. The current sensitivity was insufficient for spin-echo measurements on the weak pair signals, so coupled-pair coherence remains unresolved.
An extra peak near 520 kHz could contain contributions from weakly coupled or diffusive 13C spins. Its assignment remains uncertain. The authors also note that enriched 13C samples could increase a nuclear-spin gyroscope signal. However, gyroscope feasibility and performance require further comparison with established 14N approaches. Temperature-dependent spectral changes offer a separate route for studying spin-phonon interactions.
For material selection, the demonstrated operating point used diamond with 4.5 ppm NV centers and 1.1% natural 13C. The measurement system also required a homogeneous field near 487 G and alignment within 1 degree for polarization. The paper does not quantify performance for other NV concentrations or carbon-13 enrichment.
Materials and support
Section titled “Materials and support”The application uses an optically accessible, NV-containing CVD diamond plate for room-temperature ensemble NMR. The demonstrated sample contained 4.5 ppm NV centers and 1.1% natural-abundance 13C. 6CCVD’s diamond materials catalog lists MPCVD-grown single-crystal and polycrystalline plates and wafers up to 125 mm, while the engineering support page can be used to confirm the NV concentration, 13C abundance, geometry, and surface finish required for a custom sample.
View Original Abstract
We perform sensitive nuclear magnetic resonance (NMR) with spin ensembles that are polarized by nitrogen-vacancy (NV) centers in diamond at room temperature. Using stabilized lasers, a balanced detection, and a highly uniform magnetic field, we resolve sharp NMR features arising from multiple spin clusters. In particular, we investigate the coupling between nuclear spins and NV centers in the neutral and negatively charged states. Further, we perform high-precision NMR and coherent control of families of <a:math xmlns:a=“http://www.w3.org/1998/Math/MathML”> <a:mmultiscripts> <a:mi mathvariant=“normal”>C</a:mi> <a:mprescripts/> <a:none/> <a:mn>13</a:mn> </a:mmultiscripts> </a:math> nuclear spin ensembles in the <c:math xmlns:c=“http://www.w3.org/1998/Math/MathML”> <c:mrow> <c:mrow> <c:mo>|</c:mo> </c:mrow> <c:msub> <c:mi>m</c:mi> <c:mi>s</c:mi> </c:msub> <c:mrow> <c:mo>=</c:mo> <c:mn>0</c:mn> <c:mo>〉</c:mo> </c:mrow> </c:mrow> </c:math> level of the NV ground state. Applying an off-axis magnetic field reveals the various sites associated with the otherwise degenerate couplings of the <d:math xmlns:d=“http://www.w3.org/1998/Math/MathML”> <d:mmultiscripts> <d:mi mathvariant=“normal”>C</d:mi> <d:mprescripts/> <d:none/> <d:mn>13</d:mn> </d:mmultiscripts> </d:math> sites around the NV electronic spin, providing access to all the hyperfine tensor components. Finally, we observe spectroscopic signatures of pairs of nuclear spins coupled to the same NV center. These results are relevant for ensemble measurements of dynamical polarization that currently rely on expensive nuclear magnetic resonance systems as well as for recently proposed nuclear spin gyroscopes.
Single Crystal Cvd Diamond Plate
View Specs →
Customized Single Crystal Cvd Diamond Plate
View Specs →
Boron Doped Single Crystal Diamond Plate
View Specs →References we cover
Section titled “References we cover”- Quantum sensing enhancement through a nuclear spin register in nitrogen-vacancy centers in diamond
- 13 C hyperpolarization with nitrogen-vacancy centers in micro- and nanodiamonds for sensitive magnetic resonance applications
- Accurate hyperfine tensors for solid state quantum applications - case of the NV center in diamond
- All-optical nuclear quantum sensing using nitrogen-vacancy centers in diamond
- Entanglement of Spin-Pair Qubits with Intrinsic Dephasing Times Exceeding a Minute