USE OF GLOW DISCHARGE PLASMA FOR DEPOSITION WEAR RESISTANT CVD DIAMOND COATINGS TO CUTTING TOOLS WITH PCD
Paper details
Section titled “Paper details”| Field | Value |
|---|---|
| Journal | Voprosy atomnoj nauki i tehniki. Seriâ âderno-fizičeskie issledovaniâ |
| Published | 2026-04-14 |
| Authors | K.I. Koshevoy, E.N. Reshetnyak, V.E. Strel’nitskij, A. O. Lyamtseva, A.O. Chumak |
| DOI | 10.46813/2026-162-084 |
Diamond CVD coatings increased PCD cutting-tool wear resistance by more than 1.5 times when turning VK8 hard alloy and MK90 technical ceramics. The best VK8 result came from a 56 μm coating deposited in DC mode, whose rear wear chamfer measured 0.18 mm after 120 s. The thickest coating slightly increased machined-surface roughness, so thickness remains a wear-life versus finish trade-off.
Process and substrate preparation
Section titled “Process and substrate preparation”The authors deposited polycrystalline diamond on RNUN120400 inserts made from high-pressure-sintered synthetic diamond powder. Sintering lasted 20 s at 8 GPa and 1700 to 1750 °C. The starting powder had particles below 40 μm and was grown in an Mg-Zn-C system.
Because the substrate was already PCD, coating growth did not require the slow two-dimensional nucleation stage associated with diamond on foreign substrates.
During deposition, the H₂/CH₄ mixture was activated in a glow discharge stabilized by a transverse magnetic field. Inserts sat on the anode. The study compared DC with pulsed operation at 50 kHz and a duty cycle of 1.1.
Impurities released from the insert caused the discharge to become an arc once heating began at 600 °C. Arcing significantly reduced coating quality.
Pulsed pretreatment cleaned and heated inserts to 1070 to 1150 °C in one degassing cycle without a glow-to-arc transition. Each pulse lasted 18 μs, followed by a 2 μs pause.
DC heating required several high-temperature holds of 6 to 8 h each. The conclusion reports that DC treatment took 3 to 5 times longer.
Deposition conditions and coating structure
Section titled “Deposition conditions and coating structure”Methane concentration was 1 to 2%. Working-gas pressure ranged from 11 to 18 kPa. The methane partial pressure ranged from 2.2 × 10² to 2.7 × 10² Pa. Discharge power was 2 to 3 kW. Substrate temperature was 1070 to 1150 °C, measured with a Promin optical pyrometer.
Carbon deposition was measured gravimetrically. Coating thickness was calculated from the mass increase per unit area and spanned 17 to 56 μm.
The authors found continuous, faceted coatings across both insert centers and edges. Surface diamond crystals ranged from 10 to 60 μm. They valued this similarity because temperature gradients can jeopardize final coating homogeneity.
DC and pulsed coatings were compared at 1.25% methane, 2.2 kW, and 1070 ± 5 °C. Their deposition rates and morphologies did not differ significantly.
Coatings 40 to 50 μm thick grew at about 14 μm/h. Coatings up to 20 μm thick grew at 10 to 11 μm/h, reflecting slower initial growth. The average crystal size increased with thickness in both modes.
Turning tests and measured wear
Section titled “Turning tests and measured wear”The FT11 screw-cutting lathe tested uncoated and coated inserts during finish impact-free turning.
VK8 contains 92 wt.% WC and 8 wt.% cobalt. Its hardness is 17 GPa, or 88 HRA, and its Young’s modulus is 600 GPa. Turning used a 0.05 mm/rev feed, 0.2 mm depth, and 0.8 m/s speed.
MK90 is an Al₂O₃-based ceramic with 13.7 GPa hardness and a 320 GPa Young’s modulus. Its turning conditions were a 0.1 mm/rev feed, 0.1 mm depth, and 3.5 m/s speed.
Each insert made 1 to 2 passes along the machined surface, each lasting 60 s. MET-1 and MB9 optical microscopes measured the rear wear chamfer.
| Sample | Deposition mode | Coating thickness | Workpiece | Rear wear chamfer |
|---|---|---|---|---|
| 1 | Pulsed | 40 μm | VK8 | 0.27 mm after 120 s |
| 2 | Pulsed | 17 μm | VK8 | 0.21 mm after 120 s |
| 3 | DC | 21 μm | VK8 | 0.21 mm after 120 s |
| 4 | DC | 56 μm | VK8 | 0.18 mm after 120 s |
| 5 | DC | 27 μm | MK90 | 0.57 mm after 60 s |
An uncoated VK8 insert reached 0.27 mm wear after 60 s. Coated VK8 inserts ranged from 0.18 to 0.27 mm after 120 s.
For MK90, coating reduced the chamfer from 0.90 mm for the uncoated insert to 0.57 mm after 60 s. The authors therefore reported more than 1.5 times the wear resistance for both difficult-to-machine materials.
Sample 4 gave the best VK8 result, while Sample 1 gave the worst. Samples 2 and 3 both reached 0.21 mm after 120 s despite their different deposition modes.
Post-test coatings showed no peeling or cracking. The contact zones wore uniformly, without significant chipping or spalling. The authors treated this as evidence of strong coating adhesion.
Grain growth and surface finish
Section titled “Grain growth and surface finish”The 56 μm DC coating produced the smallest VK8 wear chamfer. The paper suggests that a several-fold increase in average crystal size may explain the slightly rougher finish. No numerical roughness value was reported.
The paper identifies several wear mechanisms for PCD. Fine-grain tools can chip individual diamond grains. Coarse-grain tools can develop intergranular cracks. High temperatures can also promote thermodynamically activated graphitization.
Earlier work cited by the authors found that about 30 μm DC coatings at 1110 to 1150 °C improved the surface quality of AK12M2MGN aluminum alloy.
The paper’s review says that the average crystal cross-section is commonly 10 to 20% of film thickness in conventional microcrystalline diamond. Nanocrystalline growth relies on secondary nucleation to limit grain size.
The cited studies list substrate nucleation treatment, inert-gas or nitrogen addition, and ion or electron bombardment as grain-control methods. Argon at 20 to 60% moved glow-discharge growth toward nanocrystalline films, compared with at least 80% in microwave discharge.
Cited morphology work also found that lamellar coating structures had lower roughness than globular structures. Without a substrate potential, the authors’ prior work produced 30 to 40 μm crystals in about 50 μm coatings. They identify argon addition and pulsed operation as possible controls for the next process step.
Limits and tool-selection guidance
Section titled “Limits and tool-selection guidance”Both DC and pulsed deposition produced similar rates and morphologies under the reported conditions. Use pulsed discharge for insert degassing and heating. Then choose coating thickness against the required wear life and surface finish.
Choose 20 to 30 μm when a balanced result is needed for VK8 and MK90. Among the tested samples, 56 μm DC gave the best VK8 wear result, but its slightly rougher finish remains a trade-off.
The reported evidence remains narrow. The new tests covered two workpieces with short passes and fixed cutting parameters for each workpiece. The paper reports no numerical roughness, error bars, replicate statistics, or quantitative adhesion test. It also found no clear correlation between wear resistance, deposition mode, and coating thickness.
Control of grain size remains unresolved. The authors do not establish one coating thickness that maximizes both wear resistance and finish for every workpiece. The reported adhesion evidence applies to the tested RNUN120400 inserts.
Materials and support
Section titled “Materials and support”The paper applies a 17 to 56 μm polycrystalline diamond CVD layer to PCD cutting inserts using glow-discharge CVD. 6CCVD’s diamond materials catalog lists MPCVD-grown polycrystalline diamond plates and wafers up to 125 mm, with a 0.1 to 500 μm thickness range that covers the reported coating. The engineering support link can support evaluation of a coating-on-insert geometry, since the catalog does not specify coated PCD inserts.
View Original Abstract
To improve the wear resistance of cutting tools equipped with inserts sintered from synthetic diamond powder, processes have been developed for synthesizing polycrystalline diamond coatings on their surface using the CVD method from H2/CH4 gas mixture in a glow discharge stabilized by a transverse magnetic field. Homogeneous coatings with a thickness of 17…56 μm and a clearly formed microcrystalline structure were obtained. A comparison was made between the DC and pulsed modes of operation of the discharge power source during the preparatory treatment of the cutting inserts surface and directly during the deposition of the coating. The advantages of the pulsed mode (frequency 50 kHz, duty cycle 1.1) at the preparatory treatment stage were revealed, which ensures rapid cleaning and heating of the cutting inserts surface to a synthesis temperature of 1070…1150 °C without the glow discharge transitioning to an arc discharge. It has been found that the deposition rate and surface morphology of coatings synthesized in pulsed and DC modes do not differ significantly. As the coating thickness increases, the average size of diamond crystals increases. It has been shown that the deposition of diamond coating increases the wear resistance of cutting tools when machining difficult-to-machine materials (ceramics, hard alloy) by more than 1.5 times. A coating with a thickness of 56 μm, deposited by DC mode, provided the tool with the greatest wear resistance when turning the VK8 hard alloy, however, the increase in diamond crystal size led to a deterioration in the quality of the machined surface due to an increase in its roughness. The feasibility of optimizing the size of diamond grains to improve the performance characteristics of the tool is discussed.
Free Standing Polycrystalline Cvd Diamond Membrane