Coherent quantum control of nitrogen vacancy spin with nanoscale magnets
Paper details
Section titled “Paper details”| Field | Value |
|---|---|
| Journal | Nature Communications |
| Published | 2026-05-28 |
| Authors | Md Fahim F. Chowdhury, Adi Jung, Léa La Spina, Ausrine Bartasyte, Samuel Margueron |
| DOI | 10.1038/s41467-026-73087-z |
A single nitrogen vacancy center in diamond was coherently driven at room temperature by a nanomagnet with lateral dimensions of 200 nm × 180 nm. The 200 nm × 180 nm device produced a Rabi frequency of about 7 MHz, while a 500 nm × 470 nm device yielded a spin echo time of 3.48 ± 0.01 μs.
Device architecture and drive mechanism
Section titled “Device architecture and drive mechanism”Surface acoustic waves from an interdigital transducer drove the nanoscale magnets. The transducer was fabricated on a 128° Y-cut, X-propagating lithium niobate substrate. Its 1480 nm wavelength design used 80 nm aluminum electrodes, 15 electrode pairs, and a 100 µm acoustic opening. The target impedance was 50 Ω, and the nominal Rayleigh-wave resonance was 2.6 GHz.
Applying microwave voltage to the IDT generated a Rayleigh wave and alternating tensile and compressive stress in each magnet. Through magnetoelastic coupling, this stress created an effective magnetic field. Magnetization oscillation through the Villari effect then produced an oscillating dipolar field near the NV center.
Free-standing cobalt magnets were patterned by electron beam lithography and metal evaporation. Each magnet had a 4 nm titanium adhesion layer and 14 nm cobalt layer. After lift-off, the elliptical magnets sat about 400 µm from the IDT fingers and 200 µm from the IDT pads. Two wire bonds on each IDT pad reduced parasitic inductance and improved coupling to the transmission line.
The NV center sat about 30 nm from the magnet surface during engaged scanning. Localization therefore concerns the near-field microwave at the NV center, not the position of the remote IDT.
NV center and measurement protocol
Section titled “NV center and measurement protocol”The defect was a single NV center in a [100]-cut 12C diamond tip with a nominal depth of about 10 nm. Its orientation was about 144° relative to the surface normal. The experiment used a quantum scanning microscope under ambient conditions.
The negatively charged defect has a spin-triplet ground level with |0⟩ and |±1⟩ branches. At zero field, the zero-field splitting was 2.87 GHz. A 5 mT bias along the NV axis produced ODMR peaks at 2.830 GHz and 2.9125 GHz. As the tip approached the magnet, the Zeeman shift decreased. This was consistent with a static magnet field opposing the applied bias. Applied fields ranged from 2 mT to 8 mT to tune the transition near the IDT resonance.
Continuous-wave ODMR located the resonant transition. For Rabi measurements, a laser initialized |0⟩, a resonant microwave pulse ran for time τ, and a second laser read out photoluminescence. Fitting the periodic bright and dark photoluminescence gave the Rabi frequency.
The spin echo sequence used π/2, 2τ, π, 2τ, and π/2 pulses. Final opposite-phase readout pulses separated |0⟩ from |−1⟩. Decay curves used a stretched exponential fit. Reported T₂ uncertainties came from the fit covariance matrix.
Rabi oscillations with smaller magnets
Section titled “Rabi oscillations with smaller magnets”All four magnet sizes produced decaying Rabi oscillations at room temperature.
| Nanomagnet | Rabi drive frequency | Bias field | Reported outcome |
|---|---|---|---|
| 2.0 µm × 1.8 µm | 2.647 GHz | 5 mT | Decaying Rabi oscillation |
| 1.0 µm × 0.9 µm | 2.599 GHz | 5 mT | Decaying Rabi oscillation |
| 500 nm × 470 nm | 2.669 GHz | 2.4 mT | Almost 28% photoluminescence contrast |
| 200 nm × 180 nm | 2.589 GHz | 5 mT | Rabi frequency of about 7 MHz |
Contrast normalized fluorescence after the microwave pulse against |0⟩ fluorescence without an RF pulse. The different resonant frequencies reflected the static stray field from each magnet along the NV axis. Size, shape anisotropy, and tip separation all contributed to that field.
Microwave power controls the gate rate
Section titled “Microwave power controls the gate rate”With the 500 nm × 470 nm magnet, the drive was fixed at 2.669 GHz under a 2.4 mT bias. The authors varied the arbitrary waveform generator voltage amplitude while keeping that frequency constant.
The measured Rabi rate rose from about 2 MHz to about 8 MHz as drive power increased. It followed the expected square-root dependence on microwave power. The reported generator voltages were measured before amplification.
The π-pulse time was the first minimum of the fitted Rabi curve. The π/2 time was halfway between the first maximum and that minimum. Both pulse times were taken from the fitted oscillation.
Spin echo coherence depends on the nanomagnet
Section titled “Spin echo coherence depends on the nanomagnet”The 500 nm × 470 nm device gave the longest measured room-temperature T₂. The spin echo measurements covered three magnet sizes.
| Nanomagnet | Spin echo frequency | Bias field | Measured T₂ |
|---|---|---|---|
| 2.0 µm × 1.8 µm | 2.647 GHz | 5 mT | 1.23 ± 0.29 μs |
| 500 nm × 470 nm | 2.669 GHz | 2.4 mT | 3.48 ± 0.01 μs |
| 200 nm × 180 nm | 2.605 GHz | 5 mT | 1.13 ± 0.17 μs |
The 200 nm spin echo used 2.605 GHz, rather than the 2.589 GHz used for its Rabi trace. Each T₂ came from a stretched-exponential fit to the spin echo decay. The uncertainty values were standard deviations from the fit covariance.
The authors suggest that room-temperature fluctuations of the nearby magnet caused the dephasing behind the spread in T₂. The 500 nm measurement used 2.4 mT, while the other two used 5 mT. Magnet size and bias field therefore changed together, and the data do not separate their effects.
Engineering implications and open questions
Section titled “Engineering implications and open questions”Conventional NV microwave excitation often uses 1 W to as high as 10 W, according to the paper’s introduction. Such extended fields can heat nearby devices, add dephasing, and drive unintended spins. The authors position the nanomagnet as a localized source with a small field footprint.
The measured 200 nm × 180 nm source is smaller than the cited 5 µm magnetic tunnel junction used for electrical NV control. Unlike film-based spin-wave and magnetoelastic drives, the single-domain nanomagnet generates a highly localized field.
Spatial selectivity was not tested between two neighboring NV centers. The IDT remained remote from the magnet, so integration of a compact local source with a qubit array remains unresolved.
The experiment did not demonstrate better energy efficiency than the current state of the art. The authors’ supplementary estimate projects up to four orders of magnitude greater efficiency for scaled devices with magnets within tens of nanometers of NV centers. That remains a theoretical projection.
The measurements cover one single-NV tip at room temperature in ambient conditions. They do not report many-qubit crosstalk, gate fidelity, or an integrated array. For diamond selection, the demonstrated geometry calls for a shallow, orientation-characterized NV center in single-crystal material. The paper does not establish the same performance for defect ensembles or other crystal orientations.
The authors also propose local strain, voltage-controlled magnetic anisotropy, and spin orbit torques as alternative drives for nanomagnets. A material plan should qualify defect depth and orientation before integrating an acoustic drive.
Materials and support
Section titled “Materials and support”The paper’s quantum scanning microscope requires a single-crystal diamond tip with one shallow NV center at a nominal depth of about 10 nm. 6CCVD’s diamond materials catalog lists MPCVD-grown single-crystal diamond plates and wafers up to 125 mm, with thickness from 0.1 to 500 micrometers. The engineering support link can review whether that material meets the paper’s [100] orientation and shallow single-NV requirements, since the experiment used purpose-fabricated scanning AFM tips.
View Original Abstract
Coherent control of the nitrogen-vacancy (NV) center in diamond is commonly achieved by microwave fields from conventional antennas, which suffer from scalability and thermal noise. Their spatially extended field profiles also limit their specificity in driving one NV spin without affecting other NV spins. Here, we investigate quantum control of a single NV center with microwave fields generated from a nanoscale magnet that is proximal to the NV center. Our results show nanoscale coherent control with high contrast Rabi oscillations using nearfield microwaves from shape anisotropic nanomagnets of lateral dimensions down to 200 $${{{\rm{nm}}}}$$, driven by surface acoustic wave (SAW) excitation. Furthermore, we show that varying the acoustic power driving such nanomagnets can achieve control over Rabi frequency. We also report spin-spin relaxation time ($${T}_{2}$$) of the NV center, measured up to 3.48$$\pm$$0.01 μs using microwave pulses generated by such nanomagnets. The use of the nanoscale magnets to implement highly localized coherent quantum control can replace thermally noisy microwave circuits and demonstrate a path to scalable quantum computing and sensing with NV-defects in diamond and other spin qubits. Microwave control of NV center spins in diamond is limited by power consumption and the degree of localization. Here, the authors report localized coherent quantum control of NV centers using surface acoustic wave-driven nanomagnets, enabling high-contrast Rabi oscillations and scalable, potentially energy-efficient spin manipulation.
Free Standing Boron Doped Diamond Pcd Film