All-optical low-field magnetometry of superconductors using NV nanodiamonds
Paper details
Section titled “Paper details”| Field | Value |
|---|---|
| Journal | Measurement |
| Published | 2026-06-06 |
| Authors | Omkar Dhungel, Saravanan Sengottuvel, Mariusz Mrózek, T. Lenz, Nir Bar‐Gill |
| DOI | 10.1016/j.measurement.2026.122080 |
Nitrogen-vacancy nanodiamonds detected superconductivity in a 200 nm YBCO thin film without microwave excitation. The fitted transition peaks were 87.5 K and 88.2 K, each with a 0.4 K full width at half maximum. At 83 K, flux penetration began at 3.64 ± 0.04 mT at the film center. The apparent edge onset occurred near 0.5 mT and was attributed to field focusing.
Cross-relaxation sensing without microwaves
Section titled “Cross-relaxation sensing without microwaves”Cross-relaxation converts changes in the local magnetic environment into changes in NV fluorescence. Resonant dipolar coupling between NV spins and nearby paramagnetic impurities increases the NV spin-lattice relaxation rate near zero field. A field sweep then produces a fluorescence dip whose position or amplitude reports the local field.
The salt-and-pepper implementation sprinkles nanodiamonds over the surface and reads their aggregate fluorescence. It uses optical excitation and detection but no microwaves. This avoids possible changes to a sample exposed to high-power microwave fields and avoids difficult microwave control on some specimens.
Submicron particles can sit close to a target and tolerate rough or fragile surfaces. Agglomerated particles increase the standoff distance to several hundred nanometers or even micrometers. The larger footprint then reduces signal amplitude and spatial resolution.
Sample preparation and optical readout
Section titled “Sample preparation and optical readout”The experiment used 140 nm carboxylated fluorescent nanodiamonds from Adamas Nanotechnologies. An aqueous suspension was drop-cast onto cover glass or the YBCO surface, then dried in ambient air. The YBCO film was 200 nm thick and rested on an Al2O3 substrate measuring 5 mm by 5 mm by 0.5 mm.
The sample sat on a Janis ST-500 helium-flow cryostat cold finger. Vacuum-compatible varnish improved thermal contact. A circular coil above the cryostat applied a field perpendicular to the sample plane and along the YBCO c-axis.
A custom widefield microscope provided 515 nm excitation at about 10 mW. A 50× objective with NA 0.45 collected the red fluorescence through a dichroic mirror onto a photodiode. The region of interest was about 120 µm by 120 µm.
Coil calibration used a test field and was cross-checked by ODMR with a 111-cut bulk diamond containing 3 ppm NV centers.
Temperature calibration of the fluorescence feature
Section titled “Temperature calibration of the fluorescence feature”The authors first characterized nanodiamonds on cover glass from 5 K to 294 K. A perpendicular background field was scanned from -6.5 to +6.5 mT in 0.2 mT steps. Extra points used 5 K steps from 70 K to 100 K. Lorentzian fits provided the cross-relaxation FWHM and contrast.
The linewidth stayed relatively constant, while contrast increased with temperature. Contrast varied by less than 0.2% from 70 K to 100 K. The linewidth-to-contrast ratio made sensitivity about a factor of two worse than at room temperature.
Contrast exceeded 1% above 70 K, and the fluorescence change at 1 mT was about 0.5%. These values established the modulation depth for the YBCO measurement.
Measuring the YBCO transition temperature
Section titled “Measuring the YBCO transition temperature”The YBCO sample was cooled without a field to 100 K. It was then cooled to 70 K at 1 K per minute while a 3 Hz square-wave field switched between 0 and 1 mT. The function generator supplied the lock-in reference. Normal-state field penetration produced an output of about 6 mV.
Below the transition, Meissner expulsion kept the fluorescence nearly constant, so the lock-in output fell close to zero. The authors smoothed the derivative with a 20-point moving average and fitted a double Gaussian. The fitted peak centers defined the transition temperature.
The fit gave peaks at 87.5 K and 88.2 K, both with 0.4 K FWHM. The authors excluded the gradual signal drop above Tc from the fit. They attributed the split peaks to oxygen inhomogeneity. The manufacturer specified 87.5 K, placing both fitted values near its reference.
Penetration field and vortex pinning
Section titled “Penetration field and vortex pinning”For field scans, the superconductor was cooled in zero field and stabilized before sweeping. The perpendicular field ran from 0 to 6.5 mT and then back to 0 mT. The penetration threshold was the first change in the shape of the fluorescence cross-relaxation feature.
At the film center, scans at 110 K and 90 K showed no forward-backward difference in the normal state. At 88 K, the authors observed flux expulsion to about 0.4 mT. Higher fields changed the fluorescence as vortices entered. At 83 K, the onset was 3.64 ± 0.04 mT, marked by a fluorescence increase above 1%.
The reverse sweep stayed constant at 83 K because vortices remained trapped as the applied field decreased. The authors related this hysteresis to vortex pinning at structural defects.
Near the film edge, the apparent onset at 83 K occurred near 0.5 mT. This was much lower than the 3.64 mT center value. The amplification became more apparent at lower temperatures. The authors attributed it to flux focusing and demagnetization near the edge.
Comparison and measurement limits
Section titled “Comparison and measurement limits”The 5 mm square film and its 200 nm thickness give an aspect ratio of 25,000. The authors therefore used a two-dimensional thin-film approximation. Screening currents from the four edges suppress the center field more strongly and focus flux near the boundary.
For a perpendicular vortex, their monopole model places the effective depth between the London penetration depth and the Pearl length. With a low-temperature λab of about 150 nm, they expected z0 of about 200 to 400 nm. The model gives a field gradient scaling of approximately |∇B| proportional to (h + z0) raised to the power -3.
The temperature dependence of the cross-relaxation feature was similar to prior bulk-diamond results cited by the authors. The observed edge-amplification shape was also consistent with earlier reports. The paper uses these as qualitative comparisons because it did not provide a local field calibration.
Geometric effects were neglected, and the center penetration field was treated as Hc1. A precise Hc1(0) and coherence length require fields of about 40 mT. The present setup reached only 7 mT, so it could not perform that measurement.
The 120 µm by 120 µm region averaged over screening-current variation, geometric imperfections, nanodiamond distribution, and laser power. The authors identify confocal microscopy as the route to smaller, defined measurement regions.
Implications for sensor and experiment design
Section titled “Implications for sensor and experiment design”The method suits samples where microwave fields are intrusive or hard to apply. Its widefield optical readout can map the field of view, which may help study vortex dynamics, thin-film heterostructures, and topological superconductors. Those extensions remain proposed applications rather than results of this experiment.
For diamond sensor selection, dispersion is as important as particle size. The 140 nm particles gave a small nominal standoff, but clustering raised it and averaged away local field structure. Uniform coverage and suppressed agglomeration should therefore be controlled before interpreting spatial resolution.
Measurements near the transition were possible with the present field range and widefield microscope. Local Hc1 estimates at low temperature would require a stronger field source. Confocal detection would also reduce spatial averaging, while the present setup could not provide the reference calibration needed for exact edge-field quantification.
View Original Abstract
We report a microwave-free, all-optical sensing approach for characterization of superconducting materials using nitrogen-vacancy (NV) centers in nanodiamonds. By implementing near-zero-field cross-relaxation magnetometry within a custom-built widefield fluorescence microscope integrated with a lock-in amplifier, we measured critical superconducting parameters including transition temperature and penetration fields by depositing nanodiamonds on a 200 nm YBa 2 Cu 3 O 7 − δ thin film. This minimally invasive, all-optical approach provides a general platform for measuring local magnetic responses in superconducting materials without the perturbative effects of traditional microwave-based sensing.
Electronic Grade Intrinsic Diamond Epitaxial Wafer H Terminated Superior 100 Mosfet Ready Substrate
View Specs →
Advanced Thermal Simulation Service Diamond Heat Spreader Performance Analysis
View Specs →
Free Standing Boron Doped Diamond Pcd Film
View Specs →References we cover
Section titled “References we cover”- Microwave-free imaging magnetometry with nitrogen-vacancy centers in nanodiamonds at near-zero field
- Near-zero-field microwave-free magnetometry with nitrogen-vacancy centers in nanodiamonds
- Excited-State Lifetime of NV Centers for All-Optical Magnetic Field Sensing
- Spin Dynamics of a Solid-State Qubit in Proximity to a Superconductor
- All-optical and microwave-free detection of Meissner screening using nitrogen-vacancy centers in diamond
Original source
Section titled “Original source”References
Section titled “References”- 2024 - Nanoscale diamond quantum sensors for many-body physics [Crossref]
- 2024 - 2024 Roadmap on magnetic microscopy techniques and their applications in materials science [Crossref]
- 2024 - Imaging the meissner effect in hydride superconductors using quantum sensors [Crossref]
- 2018 - Probing condensed matter physics with magnetometry based on nitrogen-vacancy centres in diamond [Crossref]
- 2011 - Detection of the meissner effect with a diamond magnetometer [Crossref]
- 2019 - Measuring the lower critical field of superconductors using nitrogen-vacancy centers in diamond optical magnetometry [Crossref]
- 2019 - Color centers in diamond as novel probes of superconductivity [Crossref]
- 2018 - Spatially-resolved study of the meissner effect in superconductors using NV-centers-in-diamond optical magnetometry [Crossref]
- 2014 - Diamond magnetometry of superconducting thin films [Crossref]