All-optical low-field magnetometry of superconductors using NV nanodiamonds
Paper details
Section titled “Paper details”| Field | Value |
|---|---|
| Journal | Measurement |
| Published | 2026-06-06 |
| Authors | Omkar Dhungel, Saravanan Sengottuvel, Mariusz Mrózek, T. Lenz, Nir Bar‐Gill |
| DOI | 10.1016/j.measurement.2026.122080 |
A 1 mT magnetic-field modulation revealed superconductivity in a 200 nm YBa2Cu3O7−δ film without microwaves. Transition peaks occurred at 87.5 K and 88.2 K, each with a 0.4 K full width at half maximum. At 83 K, the film center showed first flux penetration at 3.64 ± 0.04 mT. At the same temperature, the edge response began near 0.5 mT. The authors associated this response with flux focusing and vortex entry.
Experimental configuration
Section titled “Experimental configuration”The authors used commercially available 140 nm carboxylated fluorescent nanodiamonds from Adamas Nanotechnologies. An aqueous suspension was drop-cast onto cover glass and YBCO, then dried in ambient air. The YBCO film was 200 nm thick on an Al2O3 substrate measuring 5 mm × 5 mm × 0.5 mm.
The coated sample sat on a Janis ST-500 helium flow cryostat under vacuum-compatible varnish for thermal contact. The custom widefield microscope used 515 nm excitation at approximately 10 mW and a 50× objective with NA 0.45. A photodiode collected red fluorescence from a 120 µm × 120 µm region. A circular coil applied a field perpendicular to the sample plane.
The coil field was calibrated with a test field and cross-checked by ODMR on 111-cut bulk diamond containing 3 ppm NV centers. That ODMR measurement served as calibration. The operating magnetometry used no microwave.
Cross-relaxation response near zero field
Section titled “Cross-relaxation response near zero field”Cross-relaxation comes from resonant dipolar coupling between NV spins and nearby paramagnetic impurities. This coupling increases the NV spin-lattice relaxation rate when the sublevel splitting matches another spin system. The effect is strongest near zero magnetic field, where the NV orientations are degenerate. A field sweep reveals these resonances as dips in fluorescence, so their position and shape report the local environment.
The authors call their scattered-particle placement the salt-and-pepper technique. The distance between NVs inside each particle and the sample was shorter than the 140 nm particle size. Clusters can increase the standoff to several hundred nanometers or even micrometers. This reduces magnetic signal amplitude and spatial resolution by averaging over the larger footprint.
The authors scanned a perpendicular background field from −6.5 mT to +6.5 mT in 0.2 mT steps. They extracted contrast and full width at half maximum from 5 K to 294 K. Measurements were denser from 70 K to 100 K, using 5 K steps, and each feature was fitted with a Lorentzian.
The linewidth stayed relatively constant, while contrast increased with temperature. Contrast changed by less than 0.2% between 70 K and 100 K. The linewidth-to-contrast ratio made sensitivity about a factor of two worse over that range than at room temperature. The authors found this temperature behavior similar to earlier measurements on bulk diamond.
Above 70 K, cross-relaxation contrast exceeded 1%. A 1 mT field therefore produced about a 0.5% fluorescence change, enough to detect Meissner screening.
Transition temperature from fluorescence suppression
Section titled “Transition temperature from fluorescence suppression”Most cited NV studies of superconductors use ODMR, spin-lattice relaxation, or Hahn-echo methods. Those methods require microwaves, which can alter local sample properties or be difficult to apply without intrusion. The present measurement avoided both issues.
The authors modulated the perpendicular field between 0 and 1 mT at 3 Hz. They first cooled the sample to 100 K without a field. They then cooled it to 70 K at 1 K per minute. The lock-in output reached about 6 mV above the transition. Below 88 K, the output stayed close to zero because Meissner screening expelled the modulated field.
They smoothed the derivative with a 20-point moving average and fitted it with a double Gaussian. The two fitted centers were 87.5 K and 88.2 K, each with a 0.4 K full width at half maximum. The split was attributed most likely to oxygen inhomogeneity, but the paper did not test that cause directly. Both centers were consistent with the manufacturer’s stated 87.5 K transition temperature.
Flux penetration at the film center
Section titled “Flux penetration at the film center”At fixed temperatures, the authors swept the background field from 0 to 6.5 mT and back. They recorded integrated fluorescence at the film center and near an edge. At 110 K and 90 K, forward and backward traces agreed, consistent with the normal state.
At 88 K, the center expelled the applied field up to approximately 0.4 mT. A fluorescence change at higher field marked the first penetration into the mixed vortex state. At 83 K, penetration began at 3.64 ± 0.04 mT and raised fluorescence by more than 1%.
The backward trace stayed constant after the forward sweep. The authors attributed this hysteresis to vortices pinned to structural defects in the YBCO lattice. Trapped vortices kept sensing a magnetic contribution as the external field decreased.
The measured onset was treated as the penetration field. Equating it with Hc1 requires assumptions about geometry and screening currents.
Edge response and vortex pinning
Section titled “Edge response and vortex pinning”The 5 mm square film had an aspect ratio of 25,000 relative to its 200 nm thickness. This large ratio supported a two-dimensional thin-film treatment. Screening currents from four sides suppress the field most strongly at the center. Near an edge, flux focusing raises the local field and lowers the onset of vortex entry.
The edge measurement used a 120 µm diameter spot, with about 60 µm extending into the film. At 83 K, the edge showed a clear fluorescence drop near 0.5 mT. The center did not change until 3.64 ± 0.04 mT. The authors therefore identified the edge response as the mixed-state regime at a much lower applied field.
Below the transition, backward scans showed reduced fluorescence, consistent with the stronger edge response. The apparent field amplification grew as temperature decreased. The authors attributed this trend to flux focusing and demagnetization effects near the edge.
They did not determine the local amplification quantitatively. A bare-nanodiamond reference would have required field amplitudes beyond the setup.
Limits of the measurement
Section titled “Limits of the measurement”The setup reached a maximum field of 7 mT. Estimating Hc1 at zero temperature requires measurements far below Tc and fields of about 40 mT. The present geometry also neglected edge effects when identifying the center penetration field with Hc1. These limits prevent a precise Hc1 estimate and a corresponding superconducting coherence-length extraction.
The 120 µm × 120 µm widefield region averaged over screening variations, geometric imperfections, particle-density differences, and laser-power variations. A confocal microscope could probe smaller, defined regions and reduce these averaging effects.
Agglomeration remains a separate limitation because it increases the sensor-to-sample distance. The two transition peaks also leave the proposed oxygen-inhomogeneity explanation unconfirmed.
Implications for diamond sensor design
Section titled “Implications for diamond sensor design”The results identify nanodiamond particle size, dispersion, and standoff as practical sensor-design parameters. A homogeneous layer of 140 nm particles gave the short standoff needed for weak vortex and edge fields. Agglomerated particles reduced both signal amplitude and spatial resolution.
Drop-casting also allows the method to cover rough surfaces and fragile samples. Most NV magnetometers require microwave delivery and resonant spin control. The cross-relaxation readout avoids those components during measurement.
Future work could target vortex dynamics, thin-film heterostructures, and topological superconductors, but these uses remain proposals. The demonstrated requirement is a homogeneous, close-coupled nanodiamond layer on the superconducting surface.
View Original Abstract
We report a microwave-free, all-optical sensing approach for characterization of superconducting materials using nitrogen-vacancy (NV) centers in nanodiamonds. By implementing near-zero-field cross-relaxation magnetometry within a custom-built widefield fluorescence microscope integrated with a lock-in amplifier, we measured critical superconducting parameters including transition temperature and penetration fields by depositing nanodiamonds on a 200 nm YBa 2 Cu 3 O 7 − δ thin film. This minimally invasive, all-optical approach provides a general platform for measuring local magnetic responses in superconducting materials without the perturbative effects of traditional microwave-based sensing.
Electronic Grade Intrinsic Diamond Epitaxial Wafer H Terminated Superior 100 Mosfet Ready Substrate
View Specs →
Diamond Heat Spreader With Copper Coated Metalized Surface
View Specs →
Advanced Thermal Simulation Service Diamond Heat Spreader Performance Analysis
View Specs →References we cover
Section titled “References we cover”- Microwave-free imaging magnetometry with nitrogen-vacancy centers in nanodiamonds at near-zero field
- Near-zero-field microwave-free magnetometry with nitrogen-vacancy centers in nanodiamonds
- Excited-State Lifetime of NV Centers for All-Optical Magnetic Field Sensing
- Spin Dynamics of a Solid-State Qubit in Proximity to a Superconductor
- All-optical and microwave-free detection of Meissner screening using nitrogen-vacancy centers in diamond
Original source
Section titled “Original source”References
Section titled “References”- 2024 - Nanoscale diamond quantum sensors for many-body physics [Crossref]
- 2024 - 2024 Roadmap on magnetic microscopy techniques and their applications in materials science [Crossref]
- 2024 - Imaging the meissner effect in hydride superconductors using quantum sensors [Crossref]
- 2018 - Probing condensed matter physics with magnetometry based on nitrogen-vacancy centres in diamond [Crossref]
- 2011 - Detection of the meissner effect with a diamond magnetometer [Crossref]
- 2019 - Measuring the lower critical field of superconductors using nitrogen-vacancy centers in diamond optical magnetometry [Crossref]
- 2019 - Color centers in diamond as novel probes of superconductivity [Crossref]
- 2018 - Spatially-resolved study of the meissner effect in superconductors using NV-centers-in-diamond optical magnetometry [Crossref]
- 2014 - Diamond magnetometry of superconducting thin films [Crossref]