High-Output-Current Boron-Doped Single-Crystal Diamond MOSFETs with a Thin Boron-Doped Epitaxial Layer
Paper details
Section titled “Paper details”| Field | Value |
|---|---|
| Journal | Nanomaterials |
| Published | 2026-07-25 |
| Authors | Yi-Xiang Wang, Ruozheng Wang, Liangshun Qu, Genqiang Chen, Feng Wen |
| DOI | 10.3390/nano16150915 |
At 150 °C, the fabricated 500 nm boron-doped single-crystal diamond MOSFET reached a maximum drain current of −1.05 mA/mm, about 35 times the room-temperature current magnitude, while the on/off ratio stayed near 10^5. In the same temperature sweep, on-resistance fell from 413.91 to 12.13 kΩ·mm, and transconductance rose from 2.87 to 83.53 µS/mm. These results show that a thin boron-doped epitaxial channel can support stronger p-channel conduction without losing gate modulation over the measured range.
Epitaxial channel and impurity profile
Section titled “Epitaxial channel and impurity profile”The active channel was a 500 nm boron-doped single-crystal diamond epitaxial layer with a boron concentration of 10^17 to 10^18 cm⁻³. It was grown by in situ MPCVD on an intrinsic diamond epitaxial buffer. The starting substrate was 3 × 3 × 0.5 mm³ Ib-type (100) HPHT single-crystal diamond.
SIMS placed the boron-doped layer at 0 to approximately 500 nm. The intrinsic buffer extended from approximately 500 to 900 nm, where boron fell sharply. The substrate extended from approximately 900 to 1500 nm, where boron approached background. Nitrogen remained low in both epitaxial layers and rose sharply in the HPHT substrate. The authors interpret the buffer as reducing nitrogen-related influence on the upper channel.
Ring-gate fabrication and test setup
Section titled “Ring-gate fabrication and test setup”The authors chose a ring-gate structure to suppress edge leakage and increase output current. Gate lengths were 12, 8, and 4 µm. The gate width was 745 µm, and the drain electrode diameter was 200 µm.
Fabrication began with a boiling H2SO4 and HNO3 mixture at 250 °C for 1 h. The intrinsic and boron-doped layers were then grown by in situ MPCVD. A 30 min ultraviolet ozone treatment changed the hydrogen-terminated surface to oxygen termination.
The Ti/Pt/Au source-drain electrodes were 50/50/100 nm thick. Electron-gun evaporation used approximately 5 × 10⁻⁴ Pa and 1 Å/s. The contacts were annealed at 550 °C for 20 min in argon.
A 200 nm SiO2 gate dielectric and passivation layer was deposited by PECVD at 350 °C. The Ti/Au gate electrode used 50/100 nm thicknesses. Plasma etching in CF4, Ar, and O2 opened the contact windows. An Agilent B1505A semiconductor device analyzer measured the electrical characteristics.
Room-temperature output and gate control
Section titled “Room-temperature output and gate control”Output curves used gate voltages from −40.0 to 60.0 V in 5.0 V steps. All three devices showed clear p-channel operation. The principal geometry-dependent results were:
| Device | Gate length (µm) | Maximum current (mA/mm) | On-resistance (kΩ·mm) | Threshold voltage (V) |
|---|---|---|---|---|
| MOSFET-I | 12 | −0.18 | 60.24 | 133.71 |
| MOSFET-II | 8 | −0.06 | 172.41 | 71.53 |
| MOSFET-III | 4 | −0.02 | 500 | 53.82 |
Threshold voltage was extracted at VDS = −20 V by linear extrapolation of the square-root drain-current plot in the strong-conduction region. The transconductances were 6.21, 2.80, and 2.41 µS/mm for MOSFET-I, MOSFET-II, and MOSFET-III. Their on/off ratios ranged from 10^4 to 10^5.
Gate length and access spacing changed together. Shorter devices had longer access regions, which increased resistance and reduced current. The high thresholds reflect the bulk-doped channel, where residual holes require a large positive gate bias to modulate charge. Increasing boron concentration or layer thickness raises current but also raises threshold, creating a material tradeoff.
Temperature-dependent conduction
Section titled “Temperature-dependent conduction”The temperature sweep covered room temperature through 150 °C. Output curves used VGS = −40 V, and transfer curves used VDS = −20 V.
| Temperature | Current magnitude (mA/mm) | On-resistance (kΩ·mm) | Transconductance (µS/mm) |
|---|---|---|---|
| Room temperature | 0.03 | 413.91 | 2.87 |
| 50 °C | 0.05 | 188.11 | 5.32 |
| 75 °C | 0.14 | 74.05 | 12.71 |
| 100 °C | 0.32 | 33.74 | 32.30 |
| 125 °C | 0.60 | 19.82 | 52.84 |
| 150 °C | 1.05 | 12.13 | 83.53 |
The on/off ratio stayed approximately 10^5 across the measured temperatures, although VTH shifted with temperature. Hall measurements on the boron-doped layer extended from room temperature to 225 °C. Carrier concentration increased continuously, while Hall mobility decreased slightly, mainly because of enhanced phonon scattering. The authors conclude that thermal activation of boron acceptors raised the hole concentration enough to dominate transport. This concentration change may also have contributed to the threshold shift.
Breakdown and field concentration
Section titled “Breakdown and field concentration”The measured breakdown voltage was −347 V at a gate-to-drain spacing of 12.5 µm. Dividing this by the spacing gives an average lateral breakdown field of approximately 0.28 MV/cm. This is far below the paper’s cited intrinsic critical field of 10 MV/cm.
TCAD simulation at −347 V placed the peak electric field near the drain-side gate edge. The field extended toward the SiO2/B-diamond interface, so the authors infer that breakdown was not limited by intrinsic bulk diamond. The simulation used the ATLAS module of Silvaco TCAD v2018. It included transport, recombination, mobility, and impact ionization models.
Comparison with prior devices
Section titled “Comparison with prior devices”The paper does not present 500 nm as the thinnest boron-doped active layer. Its literature table lists a 230 nm device with 0.0019 mA/mm at room temperature, an on/off ratio of about 10^4, and 200 V breakdown [8]. A 700 nm device produced 0.49 mA/mm at room temperature, with a 63.2 V threshold and 18.7 µS/mm transconductance [11].
A 1,514 nm layer reported 76.9 mA/mm at 300 °C and 109.2 mA/mm at 400 °C [24]. Its thicker channel produced higher current, but the geometries and test conditions differed. The present device reached 1.05 mA/mm at 150 °C while retaining an on/off ratio near 10^5.
Nor was breakdown a record. The table lists a 150 nm device with breakdown above 1,700 V [31]. The introduction also cites a hydrogen-terminated diamond MOSFET at 1.35 A/mm and a 3,326 V breakdown. The result should therefore be read within the boron-doped, temperature-focused device class.
Engineering implications and open issues
Section titled “Engineering implications and open issues”Additional devices on the same sample showed measurable spread. Maximum current magnitudes ranged from 0.02 to 0.10 mA/mm, on/off ratios ranged from 10^3 to 10^6, and one threshold exceeded 110 V. The authors associate this spread with local boron nonuniformity, contact resistance, access spacing, and SiO2/B-diamond interface quality.
Gate leakage remained relatively low over most gate-bias values but increased at high negative gate bias. High-field fits suggest that Poole-Frenkel emission and Fowler-Nordheim tunneling may contribute. Better interface quality is needed to limit trap-assisted leakage and improve reliability.
Long-duration high-temperature operation and dielectric reliability remain untested. The authors propose geometry changes, field-plate management, and p-n heterojunctions for later work. Increasing the gate-to-drain spacing could reduce the average lateral field. Edge termination, field plates, and SiO2 thickness are also identified as controls for field crowding and dielectric reliability.
For material selection, the measured data support the 500 nm layer for conduction and gate modulation through 150 °C. They do not establish that thickness or boron concentration is optimal. The authors also expect bulk boron conduction to be less sensitive to ambient adsorbates than hydrogen-terminated channels, but they did not test that expectation over time.
Materials and support
Section titled “Materials and support”The device requires a 500 nm boron-doped single-crystal diamond channel on an intrinsic diamond buffer, with Ti/Pt/Au source-drain contacts and a Ti/Au gate. 6CCVD’s diamond materials catalog lists MPCVD-grown single-crystal and polycrystalline diamond, boron-doped diamond, and Au, Pt, and Ti metallization. Custom fabrication for this channel and contact specification can be discussed through engineering support.
View Original Abstract
High-output-current boron-doped diamond (B-diamond) metal-oxide-semiconductor field-effect transistors (MOSFETs) with a modulated boron-doped epitaxial layer were fabricated. An intrinsic diamond epitaxial layer was deposited on the single-crystal diamond substrate as a buffer layer, and plasma-enhanced chemical vapor deposition (PECVD) SiO2 was employed as both the gate dielectric and passivation layer. The boron-doped epitaxial layer has a thickness of approximately 500 nm and a boron concentration in the range of 1017-1018 cm−3. The B-diamond MOSFETs showed clear p-channel operation, with a maximum output current of −0.18 mA/mm at room temperature. When the temperature was increased to 150 °C, the maximum output current increased to −1.05 mA/mm, while the on-resistance decreased from 413.91 to 12.13 kΩ·mm. The on/off ratio remains approximately 105 over the measured temperature range. In addition, the device exhibited a breakdown voltage of −347 V at a gate-to-drain spacing of 12.5 μm, and the simulation results showed that the peak electric field was mainly concentrated near the drain-side gate edge of the passivation layer. These results indicated that, for the B-diamond MOSFETs, a balanced epitaxial layer thickness and boron concentration were essential for achieving sufficient channel conduction as well as effective gate control ability.
Electronic Grade Intrinsic Diamond Epitaxial Wafer H Terminated Superior 100 Mosfet Ready Substrate
View Specs →
Boron Doped Single Crystal Diamond Plate
View Specs →
Boron Doped Diamond On Titanium Bdd Electrode
View Specs →References we cover
Section titled “References we cover”Original source
Section titled “Original source”References
Section titled “References”- 2004 - New Unipolar Switching Power Device Figures of Merit [Crossref]
- 1993 - Device Properties of Homoepitaxially Grown Diamond [Crossref]
- 2002 - High Carrier Mobility in Single-Crystal Plasma-Deposited Diamond [Crossref]
- 2021 - Fabrication of Dual-Barrier Planar Structure Diamond Schottky Diodes by Rapid Thermal Annealing [Crossref]
- 2008 - Diamond as an Electronic Material [Crossref]
- 2021 - C-Si Bonded Two-Dimensional Hole Gas Diamond MOSFET with Normally-off Operation and Wide Temperature Range Stability [Crossref]
- 2020 - Oxidized Si Terminated Diamond and Its MOSFET Operation with SiO2 Gate Insulator [Crossref]
- 2017 - Deep-Depletion Mode Boron-Doped Monocrystalline Diamond Metal Oxide Semiconductor Field Effect Transistor [Crossref]
- 2018 - High Quality Al2O3/(100) Oxygen-Terminated Diamond Interface for MOSFETs Fabrication [Crossref]
- 2021 - Recent Progress in Deep-Depletion Diamond Metal-Oxide-Semiconductor Field-Effect Transistors [Crossref]