LiF Particles for Chemical Seeding of Diamond Films - Nucleation and Growth in Microwave Plasma CVD
Paper details
Section titled “Paper details”| Field | Value |
|---|---|
| Journal | Functional Diamond |
| Published | 2026-08-16 |
| Authors | Ivan A. Tiazhelov, Мартьянов Артём Константинович, С. В. Кузнецов, Sergey S. Savin, Alexander A. Zhivopistsev |
| DOI | 10.1080/26941112.2026.2715804 |
LiF particles produced a nearly continuous polycrystalline diamond film on aluminium nitride (AlN) after 30 minutes at 900°C and 4% CH4, without conventional nanodiamond seeding. Nucleation density increased almost linearly from 750°C to 900°C, while the growth rate reached approximately 6 µm h⁻¹ at 950°C with 4% CH4.
LiF initiated nucleation without nanodiamond seeds
Section titled “LiF initiated nucleation without nanodiamond seeds”Secondary electron SEM images showed well-faceted diamond crystallites across the AlN surface at every tested temperature. At 900°C, coalesced grains covered almost the entire surface. At 950°C, larger crystallites left wider gaps between them.
LiF residue was not visible in the SEM images after plasma treatment. The authors interpret LiF as a transient nucleation initiator that was consumed or etched. This interpretation agrees with their earlier evidence of diamond formation on or in place of the original LiF particles.
Because LiF contains no carbon, it did not supply carbon for the new diamond. The result supports chemical nucleation by a non-carbon particle.
Two process series separated temperature and methane tests
Section titled “Two process series separated temperature and methane tests”Polished polycrystalline AlN plates measured 10 × 10 × 0.38 mm and had Ra below 50 nm. Ground commercial LiF optical single crystal was suspended in DMSO at 1 mg mL⁻¹. The suspension was applied by drop casting. Each drop was 40 µL, and the resulting particle density was about 10⁷ cm⁻². The plates were dried at 150°C for 15 min.
Depositions used an ARDIS-100 microwave plasma CVD reactor at 2.45 GHz. Every run lasted 30 min with a total flow of 500 sccm. A two-color pyrometer measured substrate temperature during growth.
In the temperature series, substrate temperature was 750 to 950°C in 50°C steps at 4% CH4. Chamber pressure was 57 to 79 Torr, and microwave power was 3.8 to 4.2 kW. In the methane series, CH4 was 2 to 20% of total flow at 850°C. Pressure was adjusted over 58 to 73 Torr and power over 3.5 to 4.0 kW to hold the substrate at 850°C.
Tescan MIRA3 secondary electron images were segmented with Python-based software. The analysis divided total segmented area by mean crystallite area from representative regions. It therefore estimated density from morphology rather than directly counting every nucleus.
Temperature controlled nucleation and film continuity
Section titled “Temperature controlled nucleation and film continuity”Nucleation density increased almost linearly from 750°C through 900°C. At 900°C, increasing nucleation produced effective grain coalescence and a nearly continuous polycrystalline film after 30 min at 4% CH4.
At 950°C, nucleation density fell by approximately 6% relative to 900°C. Larger isolated crystallites and wider gaps changed the morphology to island-like growth.
The growth rate still increased and reached approximately 6 µm h⁻¹ at 950°C. Thus, the fastest measured growth did not coincide with the most continuous morphology.
In some samples, the estimated nucleation density exceeded the applied LiF density of about 10⁷ cm⁻². The authors suggest that LiF melting may have produced more than one grain per particle. That explanation was not tested directly.
Methane redirected growth and grain formation
Section titled “Methane redirected growth and grain formation”Changing CH4 from 2 to 20% at 850°C had little effect on nucleation density within experimental uncertainty. The main change occurred during crystallite enlargement.
The growth rate rose to approximately 3 µm h⁻¹ at 10% CH4 and then saturated. At 10% and higher CH4, secondary nucleation appeared on already growing crystallites. This limited grain enlargement and moved the growth regime toward nanocrystalline diamond.
At 20% CH4, SEM showed a transition from microcrystalline to nanocrystalline diamond. The result agrees with the authors’ earlier work, which placed the same transition at 20% CH4 and 850°C.
Raman data separated morphology from carbon phase content
Section titled “Raman data separated morphology from carbon phase content”Raman spectra were recorded at room temperature in confocal mode with a LabRAM HR840. A 473 nm laser was focused to about 1 µm.
All samples showed a diamond line near 1332.5 cm⁻¹. Typical full width at half maximum values were 6 to 14 cm⁻¹, while the narrowest measured line was 5.6 cm⁻¹. The 5.6 cm⁻¹ value occurred at 850°C and 2% CH4.
After baseline correction and normalization to the diamond line, software fitted the diamond, graphite D and G, and trans-polyacetylene bands. The reported sp³/sp² ratio was the diamond peak area divided by the combined D, G, and trans-polyacetylene areas. It is a fitted spectral metric rather than a direct measurement of absolute phase fractions.
Raising substrate temperature from 750 to 950°C did not noticeably change this ratio. The diamond line did broaden at higher temperatures, which the authors attribute to increased defects. The line also broadened with rising methane concentration.
In the 4% CH4 temperature series, trans-polyacetylene bands became barely distinguishable at 850°C and above. Raising CH4 caused a sharp ratio decrease at 5% and a further decline to approximately 0.02 at higher concentrations. Graphitic carbon and trans-polyacetylene contributions increased, consistent with the greater grain-boundary fraction of nanocrystalline diamond.
Chemical seeding versus nanodiamond seeding
Section titled “Chemical seeding versus nanodiamond seeding”Conventional CVD nucleation on non-diamond substrates often uses 5 to 7 nm nanodiamond particles as growth centers. The paper identifies three limitations: seed cost, uneven particle distribution, and possible degradation under aggressive hydrogen plasma.
The authors’ earlier comparison found LiF to be the most nucleation-promoting material among the tested oxides and fluorides. It produced the densest crystallite arrangement on AlN and, under selected conditions, a partially coalesced polycrystalline layer. The present study maps how temperature and methane control that response.
LiF is a model non-carbon nucleation system, not a conventional carbonaceous chemical precursor. The authors suggest this route may help develop alternative nucleation methods for microcrystalline and nanocrystalline coatings. That application remains a proposed direction.
Engineering choices and unresolved questions
Section titled “Engineering choices and unresolved questions”Within the tested AlN system, 900°C and 4% CH4 produced a nearly continuous film after 30 min. The 850°C, 2% CH4 condition gave the narrowest Raman line. At 10% CH4, secondary nucleation was already pronounced, and 20% CH4 produced a nanocrystalline structure. At 950°C, the approximately 6 µm h⁻¹ growth rate came with island-like coverage.
Process selection therefore depends on whether continuity, line width, grain size, or growth rate is the priority. The reported sp³/sp² ratio also shows the increased non-diamond carbon contribution at high methane.
Several limits remain. The study used one substrate material, one seeding material, 10 × 10 mm plates, and one 30 min deposition duration. It did not include a conventional nanodiamond control. Pressure and microwave power also varied with the process recipes, so the results do not isolate every plasma variable.
The results do not establish transfer to Fe or WC-Co substrates. The paper discusses them as difficult cases but does not test them. The work also does not report adhesion, residual stress, thermal conductivity, optical performance, or cross-sectional film structure. The proposed LiF melting explanation and transient seeding mechanism were not directly tested during growth.
Materials and support
Section titled “Materials and support”The paper’s process needs an MPCVD-grown polycrystalline diamond coating on AlN, with controlled nucleation, coalescence, and phase content. 6CCVD’s diamond materials catalog includes MPCVD-grown polycrystalline diamond plates and wafers up to 125 mm, with thickness from 0.1 to 500 micrometers. The engineering support service can define thickness, substrate, geometry, and scale-up requirements for a related coating program.
View Original Abstract
Polycrystalline diamond films and coatings are widely used in optical components, thermal management, and cutting tools. Chemical vapor deposition (CVD) is widely used for their synthesis, while the initial nucleation stage largely determines the continuity and morphology of the diamond layer. Conventional nucleation is achieved by surface seeding with nanodiamond particles. An alternative approach is chemical nucleation, extensively studied for carbon-containing precursors and polymers, whereas nucleation on non-carbon particles remains comparatively unexplored. Here, lithium fluoride (LiF) particles were used as a model non-carbon system to study diamond nucleation and subsequent growth in CH4-H2 microwave plasma CVD. Surface morphology and Raman spectroscopy showed that LiF promotes localized formation of well-faceted diamond crystallites without conventional nanodiamond seeding. Increasing the substrate temperature to 900°C produced a nearly linear increase in nucleation density and enabled the formation of nearly continuous polycrystalline films, whereas further heating to 950°C promoted island-like growth despite increasing growth rate. Methane concentration mainly affected the growth regime: at CH4 contents of 10% and higher, secondary nucleation became pronounced, suppressing crystallite enlargement and promoting the transition from microcrystalline to nanocrystalline diamond. Raman analysis showed that substrate temperature had little effect on the sp3/sp2 ratio, although the diamond Raman line broadened at higher temperatures, whereas elevated methane concentrations increased the contribution of non-diamond carbon phases. These findings suggest that non-carbon chemical nucleation can provide a new perspective on diamond formation during CVD, including the emergence of diamond nuclei under conditions where diamond remains thermodynamically metastable.
Single Crystal Cvd Diamond Plate
View Specs →
Electronic Grade Intrinsic Diamond Epitaxial Wafer H Terminated Superior 100 Mosfet Ready Substrate
View Specs →
Customized Single Crystal Cvd Diamond Plate
View Specs →References we cover
Section titled “References we cover”- Synthesis of Polycrystalline Diamond Films in Microwave Plasma at Ultrahigh Concentrations of Methane
- Isotope Effect in Thermal Conductivity of Polycrystalline CVD-Diamond - Experiment and Theory
- Progress in semiconductor diamond photodetectors and MEMS sensors