Diamondiyne - A 3D Carbon Allotrope With Mixed sp–sp 3 Hybridization
Paper details
Section titled “Paper details”| Field | Value |
|---|---|
| Journal | Angewandte Chemie |
| Published | 2026-09-14 |
| Authors | Yizhou Yang, Jie Xu, Yanyan Chen, Yu Xia, Sami Zeliouche |
| DOI | 10.1002/ange.4062963 |
Diamondiyne is the second known carbon allotrope with covalent bonding in all three dimensions. The authors synthesized amorphous carbon films containing diamondiyne crystallites over areas up to 5 cm². TEM and electron diffraction supported an asymmetric twofold interpenetrated network with a = b = 11.47 Å and c = 16.22 Å.
Network topology and interpenetration
Section titled “Network topology and interpenetration”Diamondiyne expands the diamond topology by connecting tetrahedral sp³ carbon centers through linear diyne groups. Four sp-hybridized carbons link each sp³ center, so the chemical structure contains sp and sp³ carbons in an 8 to 1 ratio. The resulting network is a carbo-mer of diamond with a larger repeating unit and a more open structure.
The ideal, noninterpenetrated crystal has face-centered cubic Fd-3m symmetry and a unit-cell edge of 16.22 Å. The synthesized material contains two interpenetrated frameworks rather than one ideal net. Their displacement is asymmetric, with the two nets separated by around 3 Å.
Interfacial cascade synthesis
Section titled “Interfacial cascade synthesis”The synthesis used a cascade reaction at a chloroform-water interface. Tetra(triethylsilylethynyl)methane and CuF₂ were distributed in separate phases, while pyridine was present in both. Fluoride from CuF₂ removed silyl protection groups and exposed terminal alkynes. Cu²⁺ catalyzed coupling between those alkynes.
The sequential deprotection and coupling released tetraethynylmethane gradually and consumed it near the interface. This arrangement mitigated the low stability of the unprotected monomer. It also confined the reaction to the region where the reactants met.
Interfacial covalent-crystal growth follows first-order kinetics with respect to monomer, whereas bulk homocoupling is expected to follow second-order kinetics. The authors used a 7 mM monomer concentration to favor molecule-by-molecule addition to a growing crystallite over cluster aggregation. Film growth proceeded normally to the interface.
NMR tracks localized monomer release
Section titled “NMR tracks localized monomer release”Deprotection was monitored by ¹H NMR in deuterated chloroform. Pyridine signals at 6.5 to 8.5 ppm increased during the first days. A terminal alkyne signal became clear after a little less than one week. The monodeprotected monomer appeared around 2.35 ppm, followed by less intense di-, tri-, and tetradeprotected species at higher shifts.
Slice-selective ¹H NMR on day 7 measured the vertical concentration profile. Slices were 1.25 mm apart. Deprotected signals were stronger near the interface, while protected signals grew farther away. Control samples showed no effect from the water phase on this signal pattern.
The persistent gradient showed that diffusion did not homogenize the chloroform phase during coupling. It supported localization of deprotection and polymerization at the interface.
Film morphology and mechanical properties
Section titled “Film morphology and mechanical properties”The films reached areas up to 5 cm² and appeared homogeneous by optical microscopy. Wrinkles arose during transfer to silicon. AFM showed a smooth surface without observable pinholes or cracks, and SEM confirmed continuity. An edge profile gave a thickness of 16 nm.
Reaction time controlled thickness over several nanometers to tens of nanometers, with a linear relationship. Films below 5 nm had limited transfer robustness. Films above 60 nm could be transferred as pieces with areas of 10⁴ to 10⁵ square micrometers. The reported reaction yield was up to 1%, and no yield optimization was performed.
Quartz crystal microbalance measurements indicated porosity, but the film mass was too small for gas isotherm analysis. The measured Young’s modulus was 2.7 GPa. This was slightly higher than the measured PMMA value and well below the 19 GPa predicted for diamondiyne. The authors linked the difference to variation in interpenetration and amorphous content.
Spectroscopy tests the chemical structure
Section titled “Spectroscopy tests the chemical structure”FTIR and Raman spectroscopy checked the reaction products and film chemistry. The film lacked the 2873 to 2956 cm⁻¹ C-H stretching band of the silyl-protected reactant. It also lacked the 3300 cm⁻¹ terminal alkyne band. These absences indicated no residual silyl groups or terminal-alkyne intermediates.
The film produced no significant carbonyl signal in the 1700 to 1725 cm⁻¹ region used to diagnose Feldman’s earlier attempts. A weak but reproducible Raman band at 2234 cm⁻¹ matched the diyne vibration of hexa-2,4-diyne at 2261 cm⁻¹. It exceeded the monomer band at 2192 cm⁻¹ and the 2094 to 2139 cm⁻¹ range reported for amorphous and silicon variants.
Solid-state ¹³C NMR gave signals from 65 to 75 ppm. The model compound gave 72.2 and 64.9 ppm for its diyne carbons. Signals at 120 ppm identified sp² carbon byproducts, while minor carbonyl signals near 220 ppm indicated few oxidized defects.
XPS found mainly carbon and oxygen at the surface. The water-exposed top surface had more oxidation than the interior measured by EDX. Only minor traces of encapsulated fluoride appeared in the film.
Electron microscopy resolves the crystal structure
Section titled “Electron microscopy resolves the crystal structure”HRTEM showed a 3.4 Å lattice periodicity, close to the predicted 3.31 Å spacing. An iDPC-STEM image showed 9.6 Å periodicity with uneven fringe spacing. The Fourier transform and nanobeam electron diffraction had a weak 222 reflection and stronger 333, 444, and 555 reflections.
That intensity pattern did not match symmetric interpenetration. It was consistent with an asymmetric twofold network displaced by around 3 Å. Diffraction along [010] agreed with the calculated pattern. An iDPC-STEM image along [133] produced a projected electrostatic potential map that matched the simulated structure.
The supported interpenetrated structure was tetragonal, with space group I4₁/amd and unit-cell parameters a = b = 11.47 Å and c = 16.22 Å. Crystallites varied, and several measured spacings exceeded the lowest-angle CuF₂ reflection. The authors therefore assigned those crystallites to the carbon film rather than encapsulated catalyst.
TEM images from films grown for 5, 14, and 21 days showed lattice fringes after 5 days. This supported direct crystallite formation rather than later self-correction.
Defect energetics favor ordered growth
Section titled “Defect energetics favor ordered growth”Computations examined a missing node that introduced a five-membered ring into an ideal diamond-topology cluster. Complete relaxation was used as the zero-energy reference. Constraining carbon atoms toward the ideal structure increased the defect energy to 18 kJ/mol and likely above. The authors related this value to a rough equilibrium constant of 10⁻³.
The estimate excludes the larger energy needed to create the defect initially. That term was not calculated because cluster models would require hydrogen end caps of different sizes. The calculations nevertheless support a growth condition that favors the intended network. Low monomer concentration and a high error penalty favor one-by-one crystal growth over cluster aggregation.
Selection implications and unresolved questions
Section titled “Selection implications and unresolved questions”The product is an amorphous carbon film containing diamondiyne crystallites, not a bulk diamondiyne crystal. Crystallite content, interpenetration, and amorphous fraction varied through the film. Porosity remained qualitative because gas sorption could not be measured on the available mass.
The evidence supports use as a synthesis and characterization platform for a new carbon allotrope. It does not establish gas storage, conductivity, optical behavior, or device-level performance. The authors did not optimize yield, and sub-5 nm films remained difficult to transfer. Those constraints matter before any application claim.
For materials selection, the 5 cm² area and linear thickness control offer useful process data. The 2.7 GPa modulus identifies the film as mechanically distinct from the 19 GPa diamondiyne prediction. A device program would need to separate signals from the crystalline domains from those of the surrounding amorphous carbon before attributing performance to diamondiyne.
View Original Abstract
ABSTRACT The creation of carbon allotropes is synthetically highly challenging, but their practical significance to science and technology cannot be underestimated. Here, we report the synthesis of a new carbon allotrope, diamondiyne, which is the second known one (after diamond) that forms covalent bonds in all three dimensions. Diamondiyne has a mixed sp-sp 3 hybridization, resulting in a carbo‐mer of diamond with an expanded diamond‐topology network. On the nanoscopic scale, two asymmetrically interpenetrated 3D networks form the tetragonal space group I 4 1 / amd with unit cell parameters a = b = 11.47 Å and c = 16.22 Å. Amorphous carbon films containing diamondiyne crystals are formed using a cascade reaction at a liquid-liquid interface. Just as for a covalent organic framework, molecular nodes are connected based on geometrical constraints to form an extended structure, and we show that the method is scalable in both the thickness and the lateral direction of the film. New carbon allotropes have historically found widespread use in materials science, and we look forward to what applications might emerge for diamondiyne.