Machinability in Turning of Aluminum Alloy Composites Reinforced with Carbonized Biocoke
Paper details
Section titled “Paper details”| Field | Value |
|---|---|
| Journal | Journal of Smart Processing |
| Published | 2026-09-10 |
| Authors | Yoshihiro TOMITA, Satoru MIZUNO, Toshiki ONARI, Takashi FUJITA, Kazunori Asano |
| DOI | 10.7791/jspmee.15.223 |
Carbonized rice husk biocoke reduced cutting resistance and finished-surface roughness in cast AC8A aluminum alloy composites. With polycrystalline diamond tools, the composites also had lower cutting resistance and smoother surfaces than a composite containing 25 vol% PAN carbon fiber. Their Rz fell below the study’s calculated theoretical roughness of 6.3 µm, while unreinforced AC8A produced an Rz slightly above it.
Composite design and reference comparison
Section titled “Composite design and reference comparison”Biocoke, abbreviated BIC, was produced from rice husk and carbonized at 643 K, 823 K, and 973 K. The carbonized BIC was infiltrated with AC8A alloy melt by squeeze casting. A PAN carbon fiber preform was infiltrated under the same conditions to provide a reference composite.
| Specimen | Reinforcement | Carbonization temperature | Reinforcement volume fraction | Turning test |
|---|---|---|---|---|
| AC8A | None | Not applicable | Not applicable | Yes |
| PAN composite | PAN carbon fiber | Not applicable | 25 vol% | Yes |
| BIC 643 K | Rice husk biocoke | 643 K | 64 vol% | No |
| BIC 823 K | Rice husk biocoke | 823 K | 63 vol% | Yes |
| BIC 973 K | Rice husk biocoke | 973 K | 56 vol% | Yes |
The carbonization temperature changed the amount of BIC retained in the composite. The reinforcement fraction decreased from 64 vol% at 643 K to 63 vol% at 823 K and 56 vol% at 973 K.
The cutting comparison used only the 823 K and 973 K composites. This choice followed an initial hardness evaluation, which found almost no hardness difference between the 643 K and 823 K specimens. The PAN composite remained the paper’s reference for a carbon fiber reinforced AC8A material.
Hardness and carbonization effects
Section titled “Hardness and carbonization effects”Unreinforced AC8A had an average Vickers hardness of about 85 HV based on measurements at ten locations. The PAN composite was harder than AC8A, while the BIC composites were less hard than both AC8A and the PAN composite.
BIC composite hardness increased with carbonization temperature, and the 973 K composite was the hardest BIC specimen. The authors proposed that higher temperatures decomposed more volatile material and increased internal porosity in the BIC. Aluminum alloy infiltration into this pore structure then increased the composite hardness.
This mechanism was an interpretation of the hardness trend rather than a direct pore measurement in the turning specimens. The similar hardnesses of the 643 K and 823 K composites also corresponded to similar reinforcement fractions of 64 vol% and 63 vol%.
Turning tests and measurement method
Section titled “Turning tests and measurement method”The authors cut ring specimens with an outside diameter of 40 mm, an inside diameter of 16 mm, and a length of 20 mm. They mounted the specimens on a manual lathe equipped with a dynamometer.
Two tool materials were compared. The H1 tool was a cemented carbide, and the PCD tool was polycrystalline diamond. Cutting resistance was recorded as the force waveform along the cutting direction. The analysis averaged 1000 consecutive measurement points from the cutting portion of each waveform.
For surface inspection, the authors ultrasonically cleaned the machined specimens and examined the finished surface with an OLS4000 laser microscope. The roughness evaluation used an 80 µm cutoff and a 645 µm evaluation length. The study reported arithmetic average roughness, Ra, and maximum height roughness, Rz.
Cutting resistance
Section titled “Cutting resistance”BIC reinforcement reduced both the mean cutting resistance and its variation width relative to unreinforced AC8A with either tool. The carbonization temperature had little effect on these results.
The H1 tests showed similar cutting resistance for the BIC and PAN carbon fiber composites. The PCD tests produced a clear separation. The BIC composite had considerably lower cutting resistance than the PAN composite.
The authors related this tool-dependent difference to how each tool responds to the workpiece. Cutting with H1 is strongly affected by plastic shear and plowing in the aluminum matrix. PCD has high hardness and wear resistance, which suppresses cutting edge deformation during the test. Its cutting resistance therefore depends more on the workpiece microstructure and friction at the tool-workpiece interface.
Surface roughness and reinforcement behavior
Section titled “Surface roughness and reinforcement behavior”PCD machining of unreinforced AC8A produced large irregularities associated with plastic flow. The PAN composite had a smaller roughness amplitude, although fine irregularities remained. The BIC composite produced a smoother profile with a more distinct tool edge shape.
The H1 tests showed the same general direction of change, but the surfaces contained more coarse irregularities. The profiles of the PAN and BIC composites were not clearly different under H1.
SEM images supported the surface observations. Reinforcement largely removed the plastic deformation visible on unreinforced AC8A after H1 machining. The PAN composite contained many carbon fiber pullout marks, which indicated local fiber withdrawal and fracture during cutting. No clear reinforcement pullout marks appeared on the BIC composite surfaces.
These observations led the authors to propose that BIC fragments and pulverizes during turning. The fragments remain on the cut surface and may spread carbon over a wider area than the PAN fibers.
Across both tools, the unreinforced AC8A Rz was slightly greater than the calculated theoretical roughness of 6.3 µm. The BIC composite Rz was smaller than this value. The authors associated that result with dispersed BIC fragments producing a finish finer than the theoretical roughness based on feed and tool nose radius.
Chip formation
Section titled “Chip formation”Unreinforced AC8A produced curled chips. BIC composite chips were as short as or shorter than those from the PAN composite, and they were sometimes finer. The 823 K and 973 K composites showed little difference in chip shape.
The authors suggested that BIC acts as a crack initiation point. This promotes chip separation and fragmentation in a manner similar to the effect reported for potassium hexatitanate short fiber in an aluminum composite. The paper provides qualitative chip observations but no numerical chip-length distribution.
Proposed lubrication mechanism
Section titled “Proposed lubrication mechanism”The cutting resistance, roughness, and chip results were attributed mainly to solid lubrication by carbon released from the BIC. The authors linked this effect to the layered crystal structure of carbon and its low shear strength.
They proposed that fractured BIC particles enter the tool-workpiece interface during cutting. Because the BIC composites contained 56 to 64 vol% reinforcement, compared with 25 vol% PAN carbon fiber, the carbon-bearing phase could cover a broader part of the interface. This wider coverage was the authors’ explanation for the lower PCD cutting resistance and smoother finish.
The paper did not measure a friction coefficient or isolate the lubrication effect from other changes in the microstructure. The proposed lubrication mechanism therefore explains the observed trends but was not confirmed through a direct interface measurement.
Engineering implications and unresolved issues
Section titled “Engineering implications and unresolved issues”Carbonized rice husk BIC offers a practical machining option for squeeze-cast AC8A composites. The clearest benefit occurred during PCD turning, where BIC composites had lower cutting resistance and better surface finish than the PAN reference composite. With H1, the two carbon reinforcements had similar cutting resistance, and their surface profiles were not clearly separated.
The 823 K and 973 K composites had similar cutting resistance, surface roughness, and chip formation. Within the tested range, machining performance alone did not favor either carbonization temperature.
The comparison has several limits. It covers one cast aluminum alloy, one squeeze-casting route, turning, two tool materials, and one specimen geometry. The results do not establish performance in milling, drilling, or other aluminum alloys. Reinforcement loading also differed substantially, so the advantage over PAN carbon fiber cannot be assigned only to the reinforcement source.
The study reports no tool-life or tool-wear result, despite discussing PCD wear resistance and possible reduction in tool wear. It also provides no life-cycle assessment or cost analysis. The authors propose BIC as a lower-cost, lower-environmental-load alternative to carbon fiber, but those claims remain unmeasured in this study. For engineers, the supported application is carbonized rice husk BIC reinforced AC8A under PCD turning, with tool life and application-specific economics still requiring validation.
View Original Abstract
This study investigates the turning machinability of cast aluminum alloy composites reinforced with rice husk Biocoke (BIC) to evaluate its potential as a sustainable alternative to conventional reinforcements such as carbon fibers.BIC was carbonized at temperatures between 643 K and 973 K and infiltrated with the aluminum alloy melt by the squeeze casting to fabricate the composites.Cutting tests using cemented carbide (H1) and polycrystalline diamond (PCD) tools were performed and demonstrated that the reinforcement with the BIC significantly reduced the cutting forces and surface roughness of the alloy.Notably, the composites exhibited the machinability exceeding that of PAN-based carbon fiber composites, particularly using the PCD tools.These results are attributed to the solid lubrication effect of carbon in the BIC.Consequently, the BIC composites can offer a lowcost, eco-friendly solution for machinable lightweight materials.
Single Crystal Cvd Diamond Plate
View Specs →
Advanced Thermal Simulation Service Diamond Heat Spreader Performance Analysis
View Specs →