Trench-type inversion-channel diamond MOSFET enabled by thermochemical etching based on C solid solution into Ni
Paper details
Section titled “Paper details”| Field | Value |
|---|---|
| Journal | Diamond and Related Materials |
| Published | 2026-09-04 |
| Authors | Yuto Nakamura, Masatsugu Nagai, Kazuki Kobayashi, Kan Hayashi, Kimiyoshi Ichikawa |
| DOI | 10.1016/j.diamond.2026.114141 |
A trench-type inversion-channel diamond MOSFET showed clear FET behavior and normally-off operation at room temperature and 300 °C. Its highest measured current density was 0.87 mA/mm at 300 °C. The authors report the first operation of this trench architecture, enabled by Ni-assisted etching that formed {111} diamond sidewalls.
Why {111} trench sidewalls were required
Section titled “Why {111} trench sidewalls were required”An inversion layer in diamond forms only on a (111) surface, so trench sidewalls must provide the required {111} planes. Conventional reactive ion etching has difficulty forming this geometry. The authors’ inversion-channel devices are inherently normally off, and their threshold voltage can be controlled through the body impurity concentration. A vertical trench structure also offers advantages over a lateral device for on-resistance per unit area and breakdown voltage.
Thermochemical etching formed the required sidewalls
Section titled “Thermochemical etching formed the required sidewalls”The etch used carbon dissolution into nickel during wet annealing in a water-vapor atmosphere. A cross-sectional test began with an HPHT type Ib (100) diamond substrate. After a 3:1 H₂SO₄/HNO₃ clean at 220 °C, the authors deposited a 400 nm Ni film by photolithography and vacuum evaporation. The film contained 50 × 50 μm² squares aligned along the diamond 〈110〉 direction.
Annealing at 1000 °C for 5 min etched beneath the Ni pattern. The Ni was removed with hot acid, and the surface was OH-terminated at 500 °C for 2 h. A 50 nm Al₂O₃ film was deposited by atomic layer deposition, followed by Ti/Au. Scanning electron microscopy and transmission electron microscopy then examined the trench section.
The outer trench expanded from 50 × 50 μm² to approximately 80 × 83 μm². The authors attribute this expansion to lateral etching caused by changes in Ni shape or partial separation during annealing. The V-shaped trench was aligned along 〈110〉. Cross-sectional SEM found internal angles of 56° and 54°. The theoretical angle is 55°, and the substrate miscut was approximately 1°. The authors used this agreement to identify the sidewalls as {111} planes.
The MOSFET used a doped epitaxial diamond stack
Section titled “The MOSFET used a doped epitaxial diamond stack”The device began with a lightly boron-doped HPHT type IIb (100) substrate. MPCVD grew an N-doped layer, then heavily B-doped p⁺ layers were deposited on the front and back. Secondary ion mass spectrometry measured [B] = 3 × 10¹⁷ cm⁻³ in the substrate. It measured [N] < 1 × 10¹⁶ cm⁻³ in the n-type layer and [B] = 6 × 10¹⁹ cm⁻³ in the p⁺ layer. The n-type and p⁺ layers were 13.5 μm and 1.6 μm thick.
A 300 nm Ni pattern of 30 × 30 μm² squares aligned along 〈110〉 was applied. Wet annealing at 950 °C for 17 min formed the first trenches. Hydrogen plasma in the MPCVD system smoothed the trench sidewalls. Ni-assisted annealing at 900 °C for 20 min removed p⁺ between adjacent devices and reached the n-type layer.
After Ni removal, the authors H-terminated the surface at 850 °C for 1 h in 4% H₂/Ar. They say this mitigates residual oxygen at the Al₂O₃/diamond interface, which could raise the interface-state density after OH termination. They then OH-terminated the surface at 500 °C for 2 h and deposited 50 nm Al₂O₃ by ALD at 300 °C.
Buffered hydrofluoric acid selectively removed Al₂O₃ from the source region after photolithography. Vacuum evaporation formed Ti/Au source and gate electrodes with thicknesses of 30/120 nm. After backside cleaning, a Ti/Au drain electrode with the same 30/120 nm thicknesses was deposited. The established inversion-layer process formed the channel along the trench {111} sidewalls.
Trench geometry set the channel dimensions
Section titled “Trench geometry set the channel dimensions”The final trench was V-shaped and approximately 64 μm deep. The authors defined the channel width as the 371 μm trench periphery. They calculated a 16.5 μm channel length from the n-layer thickness and the 55° trench angle.
Cross-sectional TEM of the test sample showed that the Al₂O₃ and metal layers were uniform on the (100) and {111} surfaces. The metal was discontinuous at convex features on the trench sidewall.
Microscopy showed many surface pits after p⁺ growth. Images before and after growth linked the pits to boron-doped epitaxy rather than hydrogen-plasma treatment. Heavy boron growth can produce pits at different trimethylboron concentrations, which the authors cite as the likely cause.
Electrical performance and comparison with earlier devices
Section titled “Electrical performance and comparison with earlier devices”The I_D-V_DS curves showed clear FET behavior and current saturation at both temperatures. Threshold voltage was extracted by linear extrapolation from the point of maximum transconductance. The active area was 8073 μm², based on the trench top view.
| Condition | Maximum current density | Active-area current density | Specific on-resistance | Threshold voltage |
|---|---|---|---|---|
| Room temperature | 0.53 mA/mm | 2.3 A/cm² | 3.5 Ω·cm² | -4.9 V |
| 300 °C | 0.87 mA/mm | 4.1 A/cm² | 1.3 Ω·cm² | -6.2 V |
The on/off current ratio was approximately 3.5 orders of magnitude at room temperature. The authors attribute the likely leakage current to dislocations. At 300 °C, the higher current was attributed to increased activation of B acceptors, which reduced drift resistance.
Earlier trench diamond MOSFETs used H termination or Si termination. H-terminated devices normally conduct because they use a p-type conductive channel instead of an inversion layer. The authors describe stable normally-off operation in Si-terminated diamond MOSFETs as difficult.
An earlier inversion-channel diamond MOSFET operated on a surface etched by C solid-solution reaction in an H₂/Ar atmosphere. The new result confirms similar operation after thermochemical etching in water vapor. A prior vertical trench diamond MOSFET reported 580 V breakdown. The present paper does not report a breakdown voltage for the new inversion-channel device. The data therefore demonstrate trench channel operation rather than a direct breakdown comparison.
Sidewall steps and drift resistance set the next process targets
Section titled “Sidewall steps and drift resistance set the next process targets”Steps interrupted the gate metal and can hinder inversion-layer formation under gate bias. If present in the channel region, these interruptions would reduce current density. Steps in the channel region can also induce interface states.
The authors call atomically flat sidewalls ideal and state that etch optimization can, in principle, produce them. Dislocations inherited from the epitaxial substrate degrade sidewall flatness, so a low-dislocation substrate is required.
The lightly B-doped substrate reduced dislocation density but left a drift layer of approximately 300 μm. This thick layer increased series resistance. The authors hope that future high-quality p⁺ substrates will support a more suitable drift-layer design. Reducing the n-layer thickness could further lower channel resistance. Process optimization must therefore address both trench topography and the epitaxial drift structure.
Materials and support
Section titled “Materials and support”The application needs boron-doped diamond for the substrate and p⁺ layers, nitrogen-doped diamond for the n-type layer, and Ti/Au metallization for the gate, source, and drain. The 6CCVD diamond materials catalog includes boron-doped diamond and metallization with Au or Ti. The engineering support page can be used to discuss custom geometry and fabrication requirements for this MOSFET.
View Original Abstract
Trench-type inversion-channel diamond MOSFETs have ultimate potential as low-loss power devices, and their practical realization is highly anticipated. The fabrication of this device requires the formation of diamond trenches with {111} sidewalls because inversion layers can only be formed on diamond {111} surfaces. However, conventional etching techniques such as reactive ion etching (RIE) face difficulties in forming such structures. In this study, we achieved the formation of diamond trenches with {111} sidewalls in a doped diamond multilayer structure by employing our thermochemical etching technique. Furthermore, by applying our inversion-layer formation technique, we realized the formation of an inversion-channel on the trench sidewalls. As a result, we fabricated a trench-type inversion-channel diamond MOSFET and demonstrated its operation for the first time. The fabricated device showed clear FET characteristics and normally-off behavior at both room temperature and 300 °C. These results establish an important foundation for the realization of ultra-low-loss diamond power devices.
Electronic Grade Intrinsic Diamond Epitaxial Wafer H Terminated Superior 100 Mosfet Ready Substrate
View Specs →
Boron Doped Diamond On Titanium Bdd Electrode
View Specs →
Boron Doped Diamond Electrode On Niobium Bdd Nb Electrode
View Specs →References we cover
Section titled “References we cover”- Conductive-probe atomic force microscopy and Kelvin-probe force microscopy characterization of OH-terminated diamond (111) surfaces with step-terrace structures
- Inversion channel diamond metal-oxide-semiconductor field-effect transistor with normally off characteristics