Skip to content

Coherent control of a nitrogen-vacancy center spin ensemble with a diamond mechanical resonator

MetadataDetails
Publication Date2015-03-04
JournalOptica
AuthorsE. R. MacQuarrie, Tanay A. Gosavi, A. M. Moehle, Nicholas R. Jungwirth, Sunil A. Bhave
Citations94
AnalysisFull AI Review Included
  • Breakthrough Demonstration: First-ever coherent mechanical control of a nitrogen-vacancy (NV) center spin ensemble in single-crystal diamond using a high-overtone bulk acoustic resonator (HBAR), achieving Rabi frequencies up to Ωmech/2π ≈ 3.8 MHz.
  • Forbidden Transition Access: The mechanical drive is parity nonconserving, enabling direct access to the magnetically forbidden Δms = ±2 spin transition between |−1⟩ and |+1⟩ states.
  • HBAR Architecture: ZnO piezoelectric films (1.8 µm and 2.5 µm) sandwiched between patterned Al electrodes and Ti/Pt ground planes, sputtered directly onto bulk single-crystal diamond substrates.
  • Coherence Metrics: Mechanically driven |−1⟩ ↔ |+1⟩ qubit achieved T2* = 0.45 ± 0.05 µs, comparable to magnetically driven measurements of the same subspace.
  • Material Selection: Type IIa, h100i “optical grade” single-crystal diamond from Element Six, specified for nitrogen impurities <1 ppm with native NV ensemble densities of ~110-120 NV/µm³.
  • Δ-System Innovation: Demonstrates a phase-sensitive three-level Δ-system in the NV ground state, enabling future applications in quantum optomechanics, phase-controlled spin-phonon switches, and inertial sensing.
  • Engineering Path Forward: Identified improvements include higher Q-factor devices, higher electronic purity diamond, and engineered NV planes to eliminate driving-field inhomogeneity dephasing.
ParameterValueUnitContext
Zero-field splitting (D0/2π)2.87GHzNV ground state Hamiltonian
NV gyromagnetic ratio (γNV/2π)2.8MHz/GMagnetic field coupling
Perpendicular stress coupling (ε�/2π)0.015MHz/MPaStrain-spin interaction
Axial stress coupling (ε∥/2π)0.012MHz/MPaStrain-spin interaction
Hyperfine parameter (P/2π)−4.945MHz14N nuclear coupling
Hyperfine parameter (A∥/2π)−2.166MHz14N nuclear coupling
Mechanical mode frequency (Sample A)771MHzLow-Q HBAR resonance
Mechanical mode frequency (Sample B)529MHzHigh-Q HBAR resonance
Quality factor (Sample A)1,400—Bulk acoustic resonance
Quality factor (Sample B)4,000—Bulk acoustic resonance
Rabi frequency (Sample A, 33 dBm)1.0MHzMechanically driven
Rabi frequency (Sample B, 33 dBm)3.8MHzMechanically driven
ZnO film thickness (Sample A)1.8µmPiezoelectric transducer
ZnO film thickness (Sample B)2.5µmPiezoelectric transducer
NV center density (Sample A)~110NV/µm³Native ensemble
NV center density (Sample B)~120NV/µm³Native ensemble
Nitrogen impurity specification<1ppmType IIa optical grade
T2* (mechanical, |−1⟩↔|+1⟩)0.45 ± 0.05µsMechanical Ramsey
T2* (magnetic, |−1⟩↔|+1⟩)0.36 ± 0.09µsMagnetic Ramsey
T2* (magnetic, |0⟩↔|−1⟩)0.91 ± 0.02µsMagnetic Ramsey
T2* (magnetic, |+1⟩↔|0⟩)0.92 ± 0.02µsMagnetic Ramsey
Input microwave power33dBmHBAR drive level
Diamond crystal orientationh100i—Substrate specification
Loop antenna frequency~2.87GHzMagnetic control (spin resonance)
  • Substrate Selection: Type IIa h100i single-crystal diamond with <1 ppm nitrogen; native NV ensemble used without additional implantation.
  • HBAR Fabrication: ZnO piezoelectric film (1.8 µm or 2.5 µm) sputtered between a patterned Al electrode and a Ti/Pt ground plane on one diamond face.
  • Apodized Geometry: Diamond HBAR shape apodized to suppress lateral mechanical modes and concentrate acoustic energy in the bulk thickness mode.
  • Resonator Characterization: Microwave reflection (S11) measurements with a vector network analyzer to identify and characterize the mechanical resonance frequencies and Q-factors.
  • Mechanical Rabi Protocol (Low-Q): Optical polarization into |0⟩ → magnetic π pulse to |−1⟩ → mechanical Rabi pulse of variable length τ → second magnetic π pulse → fluorescence readout of |0⟩ population.
  • Mechanical Rabi Protocol (High-Q): Fixed-duration mechanical pulse (L = 3 µs) bracketed by short (~30 ns) magnetic π pulses; sweeping the magnetic interval through the mechanical pulse generates Rabi oscillations.
  • Ringing Modeling: Mechanical pulse modeled with ringup (1 − e−t/τr) and ringdown (e−(t−t0)/τr) functions, where τr = 2Q/ωm.
  • Ramsey Sequence: T2* extracted from exponential decay envelopes; mechanical Ramsey compared directly with magnetic Ramsey for three qubit subspaces.
  • Focal Depth Variation: Rabi oscillations measured at multiple depths inside the diamond to map stress-wave amplitude distribution within the confocal point-spread function.

This research relies on Optical Grade Single Crystal Diamond (SCD) in the h100i orientation—the same geometry used in 6CCVD’s standard product line. Specifically:

  • Optical Grade SCD (h100i): Matches the paper’s Type IIa specification with native NV density compatible with ensemble measurements. 6CCVD supplies SCD in thicknesses from 0.1 µm to 500 µm, enabling direct use as HBAR substrates.
  • Ultra-Low Nitrogen SCD: For replication with reduced spin-bath dephasing (the paper explicitly identifies “higher electronic purity diamond” as a path to improved T2*), 6CCVD can provide customized low-nitrogen-content SCD substrates.
  • Engineered NV-Density SCD: For experiments targeting single-spin or plane-of-NV geometries to eliminate driving-field inhomogeneity, 6CCVD offers consultation on nitrogen implantation and controlled NV creation protocols.
  • Custom HBAR Substrate Dimensions: The paper uses bulk diamond substrates as acoustic Fabry-Pérot cavities. 6CCVD’s capability for plates/wafers up to 125 mm (PCD) and custom SCD dimensions supports resonator fabrication at virtually any lateral scale.
  • Metallization for HBAR Electrodes: The paper’s Ti/Pt ground plane and patterned Al electrode structure can be fabricated directly through 6CCVD’s internal metallization service (Ti, Pt, Au, Pd, W, Cu available).
  • Surface Polishing for Acoustic Q: The paper notes that device Q-factor improvements of at least 5× are expected from fabrication refinements. 6CCVD’s SCD polishing capability (Ra < 1 nm) and inch-size PCD polishing (Ra < 5 nm) directly address the surface-roughness-limited acoustic loss mechanism.
  • Laser Cutting and Shaping: Apodized HBAR geometries (used to suppress lateral modes) can be produced via 6CCVD’s laser cutting and custom shaping services.

6CCVD’s in-house PhD team can assist with material selection for hybrid quantum systems requiring:

  • High-Q bulk acoustic resonators for spin-phonon coupling experiments
  • NV center ensemble substrates for magnetometry, optomechanics, or Δ-system research
  • Low-strain, high-purity diamond for coherent spin control applications
  • Custom metallization stacks (Ti/Pt/Au, Ti/Al, etc.) compatible with piezoelectric transducer fabrication

For custom specifications, material consultation, or metallization design for hybrid quantum device fabrication, visit 6ccvd.com or contact our engineering team directly.

View Original Abstract

Coherent control of the nitrogen-vacancy (NV) center in diamond’s triplet spin state has traditionally been accomplished with resonant ac magnetic fields. Here, we show that high-frequency stress resonant with the spin state splitting can also coherently control NV center spins. Because this mechanical drive is parity non-conserving, controlling spins with stress enables direct access to the magnetically forbidden |−1〉↔|+1〉 spin transition. Using a bulk-mode mechanical microresonator fabricated from single-crystal diamond, we apply intense ac stress to the diamond substrate and observe mechanically driven Rabi oscillations between the |−1〉 and |+1〉 states of an NV center spin ensemble. Additionally, we measure the inhomogeneous spin dephasing time (T2*) of the spin ensemble within this {−1,+1} subspace using a mechanical Ramsey sequence and compare it to the dephasing times measured with a magnetic Ramsey sequence for each of the three spin qubit combinations available within the NV center ground state. These results demonstrate coherent control of a spin with a mechanical resonator and could lead to the creation of a phase-sensitive Δ-system inside the NV center ground state with potential applications in quantum optomechanics and metrology.