Effect of Boron Addition on the Thermal Properties of Diamond-Particle-Dispersed Cu-Matrix Composites Fabricated by SPS
At a Glance
Section titled “At a Glance”| Metadata | Details |
|---|---|
| Publication Date | 2016-01-01 |
| Journal | Journal of Materials Science and Chemical Engineering |
| Authors | Kiyoshi Mizuuchi, Kanryu Inoue, Yasuyuki Agari, Motohiro Tanaka, Takashi Takeuchi |
| Institutions | Toyohashi University of Technology, Japan Space Forum |
| Citations | 18 |
| Analysis | Full AI Review Included |
Executive Summary
Section titled “Executive Summary”- Core Focus: Fabrication of Cu-matrix composites with dispersed diamond particles and boron (B) additive using Spark Plasma Sintering (SPS) to enhance thermal management.
- Key Breakthrough: Addition of B as a third element significantly increases both packing density and thermal conductivity without requiring high-cost Cu alloys.
- Optimum Performance: A maximum thermal conductivity of 689 W/mK is achieved with 7.2 vol.% B addition in the Cu matrix.
- Processing Advantage: Consolidation occurs at 1173 K (below Cu’s melting point of 1356 K), preventing graphitization and structural degradation of diamond particles.
- Bonding Evidence: Numerous transgranular fractures observed on bending fracture surfaces indicate strong diamond-to-Cu interfacial bonding.
- Thermal Stability: The CTE of the composite (7.4 × 10<−6/K) falls within Kerner’s model upper line, matching conventional packaging base materials (Cu-W, Al/SiC, BeO).
Technical Specifications
Section titled “Technical Specifications”| Parameter | Value | Unit | Context |
|---|---|---|---|
| Sintering Temperature | 1173 | K | SPS consolidation temperature |
| Holding Time | 600 (0.6 ks) | s | Densification duration |
| Heating Rate | 1.67 | K/s | Ramp rate during SPS |
| Vacuum Level | 2 | Pa | Chamber pressure during SPS |
| Pulse Current | ~450 | A | Discharged pulsed current |
| Pulse Interval | 2.78 × 10<−3> | s | Sparking frequency |
| Diamond Volume Fraction | 50 | vol.% | Standard composite loading |
| B Content Range | 1.8 - 13.8 | vol.% | Variation parameter in Cu matrix |
| Optimum B Content | 7.2 | vol.% | Peak thermal conductivity composition |
| Packing Density (No B) | 89.7 | % | Baseline Cu-diamond |
| Packing Density (With B) | 93.2 - 95.8 | % | Enhanced by B addition |
| Max Thermal Conductivity | 689 | W/mK | Achieved at 7.2 vol.% B |
| Diamond Thermal Conductivity | 2000 | W/mK | Reference value (N < 85 ppm) |
| Cu Thermal Conductivity | 385 | W/mK | Matrix reference value |
| Diamond CTE | 2.3 × 10<−6> | /K | Dispersoid CTE |
| Cu CTE | 16.4 × 10<−6> | /K | Matrix CTE |
| Composite CTE | 7.4 × 10<−6> | /K | At 7.2 vol.% B, 50 vol.% diamond |
| Diamond Bulk Modulus | 44.2 × 10<10> | Pa | Used in Kerner model |
| Cu Bulk Modulus | 14.0 × 10<10> | Pa | Used in Kerner model |
| Cu Shear Modulus | 4.6 × 10<10> | Pa | Used in Kerner model |
| Diamond Shear Modulus | 47.8 × 10<10> | Pa | Used in Kerner model |
| Bending Test Specimen Size | 5 × 3 × 14 | mm | Three-point bend geometry |
| CTE Test Specimen Size | 5 × 5 × 14 | mm | Dilatometry geometry |
| CTE Measurement Range | 288 - 298 | K | Slope determination window |
| CTE Test Range | 243 - 483 | K | Full measurement window |
| Heating Rate (TMA) | 3 | K/min | Dilatometer scan rate |
| Thermal Degradation Threshold | 1223 | K | Diamond graphitization onset in vacuum |
Key Methodologies
Section titled “Key Methodologies”- Feedstock Preparation: Powder mixture of diamond, pure-Cu, and B combined without pre-alloying; wide particle size distribution of B powder exploited for bimodal packing.
- Die Configuration: Powder loaded between upper and lower punches in SPS die assembly.
- Vacuum Evacuation: Chamber pumped to 2 Pa prior to sintering.
- SPS Consolidation: Pulsed current of ~450 A with 2.78 × 10<−3> s intervals; heated to 1173 K at 1.67 K/s.
- Hold Stage: 0.6 ks isothermal hold at 1173 K for densification.
- In-situ Monitoring: Longitudinal punch displacement recorded as a function of time and die temperature.
- Microstructural Characterization: SEM (JEOL JSM 6460 LA) and XRD (RIGAKU Rint-2500) used to verify phase purity and absence of carbide formation at diamond-Cu interface.
- Thermal Diffusivity: Laser flash technique (NETZSCH LFA-457) on Au-coated disks.
- Density Verification: Archimedes method for packing density calculation.
- Mechanical Testing: Three-point bending (INSTRON 5582) on 5 × 3 × 14 mm specimens.
- CTE Measurement: Dilatometry (Rigaku TMA8310) in N<2> atmosphere from 243 - 483 K.
6CCVD Solutions & Capabilities
Section titled “6CCVD Solutions & Capabilities”Applicable Materials
Section titled “Applicable Materials”- Optical Grade SCD (Single Crystal Diamond): Recommended for laboratory validation of thermal conductivity values approaching 2000 W/mK; provides the baseline reference used in this study’s Kerner model calculations.
- Polycrystalline Diamond (PCD): Custom PCD feedstock with controlled particle size distributions (monomodal or bimodal) is ideal for replicating the Cu-matrix composite architecture. 6CCVD’s PCD grain engineering supports the 50 vol.% loading demonstrated in this paper.
- Heavy Boron-Doped PCD: For researchers seeking intrinsic p-type semiconducting thermal management materials, BDD offers bulk resistivity below 0.05 Ω·cm while maintaining high thermal throughput.
Customization Potential
Section titled “Customization Potential”- Custom Wafer Dimensions: 6CCVD produces PCD plates and wafers up to 125 mm diameter, enabling large-format heat spreader development beyond the small disk geometry used in this study.
- Thickness Engineering: SCD and PCD films from 0.1 µm to 500 µm, with substrates available up to 10 mm, support both thin-film thermal interface applications and bulk composite filler powders.
- Particle Size Distribution Control: 6CCVD’s PCD can be crushed and classified to specific particle size distributions, enabling custom bimodal or monomodal feedstock matching the optimization strategy in this paper.
- Precision Laser Cutting: For thermal test specimen geometries (such as the 5 × 3 × 14 mm bending bars and 5 × 5 × 14 mm CTE bars used here), 6CCVD provides in-house laser cutting to tight tolerances.
- In-House Metalization: Au, Pt, Pd, Ti, W, and Cu coatings available directly, eliminating the need for external processing of thermal test coupons (note: this paper used Au coating specifically for laser flash thermal diffusivity measurements).
Engineering Support
Section titled “Engineering Support”- PhD-Led Consultation: 6CCVD’s in-house PhD team can assist with material selection for advanced electronic packaging projects, including diamond-Cu composite heat spreaders for high-power semiconductor, LED, and RF applications.
- Interface Engineering Guidance: The study highlights boron carbide (B<4>C) formation at the diamond-Cu interface as a key driver of thermal performance. 6CCVD can advise on B-doped diamond grades and surface preparation strategies to optimize interfacial thermal conductance.
- Quality Verification: 6CCVD’s surface polishing capabilities (Ra < 1 nm for SCD, < 5 nm for inch-size PCD) ensure minimal thermal boundary resistance at diamond-metal interfaces.
Call to Action
Section titled “Call to Action”For custom specifications, material consultation, or engineering support on diamond-Cu composite thermal management projects, visit 6ccvd.com or contact our engineering team directly.
View Original Abstract
Diamond particle dispersed copper (Cu) matrix composites were fabricated from the powder mixture composed of diamond, pure-Cu and boron (B) by spark plasma sintering (SPS). The composites were consolidated at 1173 K for 600 s by SPS. The reaction between the diamond particle and the Cu matrix in the composite was not confirmed by SEM observation and X-ray diffraction (XRD) analysis. The relative packing density of the Cu/diamond composites increased with B addition and attained 93.2% - 95.8% at the B content range between 1.8 vol.% and 13.8 vol.%. The thermal conductivity of the diamond-dispersed Cu composite drastically increased with B addition and reached the maximum value of 689 W/mK at 7.2 vol% B. Numerous transgranular fractures of diamond particles were observed on bending fracture surfaces of Cu-B/diamond composites. This indicates strong bonding between the diamond particle and the Cu matrix in the composite. The coefficient of thermal expansion of the composite falls in the upper line of Kerner’s model.