Large-scale GaP-on-diamond integrated photonics platform for NV center-based quantum information
At a Glance
Section titled “At a Glance”| Metadata | Details |
|---|---|
| Publication Date | 2016-01-13 |
| Journal | Journal of the Optical Society of America B |
| Authors | Michael N. Gould, Srivatsa Chakravarthi, Ian Christen, N. Thomas, Shabnam Dadgostar |
| Institutions | University of Washington, Yale University |
| Citations | 34 |
| Analysis | Full AI Review Included |
Technical Documentation & Analysis: GaP-on-Diamond Integrated Photonics for NV Center Quantum Information
Section titled “Technical Documentation & Analysis: GaP-on-Diamond Integrated Photonics for NV Center Quantum Information”This document analyzes the research paper “A Large-Scale GaP-on-Diamond Integrated Photonics Platform for NV Center-Based Quantum Information” to provide technical specifications and demonstrate how 6CCVD’s advanced MPCVD diamond solutions can support and scale this critical quantum technology.
Executive Summary
Section titled “Executive Summary”- Scalable Quantum Platform: The research successfully demonstrates a hybrid GaP-on-Diamond integrated photonics platform suitable for Measurement-Based Quantum Computation (MBQC) utilizing Nitrogen-Vacancy (NV) centers.
- High Efficiency Projection: The platform achieves a projected Total Quantum Efficiency (TQE) of 33% into an on-chip guided mode, representing a factor of >200 improvement over current free-space collection techniques.
- Material System: The system relies on high-quality, electronic-grade Single Crystal Diamond (SCD) substrates hosting near-surface NV centers (~15 nm deep), overlaid with a 125 nm GaP waveguiding layer.
- High Component Yield: Demonstrated high yields for key integrated components, including 89% for full measurement loops and 58% for waveguide-coupled disk resonators, confirming the platform’s suitability for complex circuit integration.
- Exceptional Quality Factors: Measured intrinsic Quality Factors (Qi) up to 11,700 in disk resonators, crucial for achieving significant Purcell enhancement (Fp ~24) and efficient ZPL photon emission.
- 6CCVD Value Proposition: 6CCVD provides the necessary high-purity, electronic-grade SCD substrates with custom dimensions (up to 125 mm) and precision thickness control required to scale this technology from lab prototypes to commercial quantum circuits.
Technical Specifications
Section titled “Technical Specifications”The following hard data points were extracted from the analysis of the integrated photonics platform performance:
| Parameter | Value | Unit | Context |
|---|---|---|---|
| Diamond Substrate Grade | Electronic Grade | N/A | Commercially sourced SCD |
| NV Center Depth | ~15 | nm | Below diamond surface (via implantation/annealing) |
| GaP Waveguide Thickness | 125 | nm | Epitaxially grown layer |
| Diamond Pedestal Etch Depth | 600 | nm | Etched into the SCD substrate |
| Resonator Intrinsic Quality Factor (Qi) | Up to 11,700 | N/A | Coupler Type 3 geometry |
| Resonator Measured Q (Best Device) | 5,100 | N/A | Used for ZPL photon collection |
| Projected On-Chip TQE | 33 | % | Into useful waveguide modes |
| Projected Off-Chip TQE | 5.5 | % | Total quantum efficiency (with grating coupler) |
| ZPL Wavelength | 637.2 | nm | Zero-Phonon Line |
| Average Grating Coupler Efficiency | 17.0 ± 1.5 | % | At ZPL wavelength |
| Directional Coupler Excess Loss (180 nm ridge) | 0.063 ± 0.015 | dB/µm | Per unit length |
| Full Measurement Loop Yield | 89 | % | 97 out of 109 loops working |
Key Methodologies
Section titled “Key Methodologies”The fabrication process relies heavily on precise material preparation and etching of the diamond substrate:
- NV Center Creation: Electronic grade diamond chips (2 mm x 2 mm) were subjected to ion implantation and annealing to create negatively charged NV centers approximately 15 nm below the surface.
- Surface Preparation: The diamond was rigorously cleaned using a solution of KNO3 in fuming H2SO4, followed by treatment with hexamethyldisilazane (HMDS) vapor.
- GaP Membrane Transfer: A 125 nm thick GaP layer, grown on an Al0.8Ga0.2P sacrificial layer, was released via wet etching (1.5% hydrofluoric acid) and transferred to the prepared diamond surface.
- Photonic Patterning: Electron-beam lithography was used with hydrogen silsesquioxane (HSQ) negative resist to define the integrated photonic structures.
- Substrate Etching (RIE): A two-step Reactive Ion Etch (RIE) was performed:
- Cl2/N2/Ar chemistry etched the GaP layer.
- O2 RIE followed, etching approximately 600 nm into the diamond substrate to form the diamond pedestal supporting the GaP waveguides.
- Measurement: Transmission measurements were conducted using a custom microscope setup, coupling light via grating couplers and analyzing output via a spectrometer or photodetector. NV emission was excited using a 532 nm laser at low temperature (T ≈ 7K).
6CCVD Solutions & Capabilities
Section titled “6CCVD Solutions & Capabilities”6CCVD is uniquely positioned to supply the foundational diamond materials and custom processing required to scale this high-performance GaP-on-Diamond quantum platform.
Applicable Materials
Section titled “Applicable Materials”To replicate and extend this research, 6CCVD recommends the following materials:
- Optical Grade Single Crystal Diamond (SCD): Required for the substrate, ensuring ultra-low birefringence and high transmission at the ZPL wavelength (637.2 nm). Our SCD offers Ra < 1 nm polishing, critical for minimizing scattering losses at the GaP/Diamond interface.
- Electronic Grade SCD Substrates: Essential for hosting high-coherence NV centers. 6CCVD provides high-purity SCD material suitable for subsequent ion implantation and high-temperature annealing protocols.
- Custom Thickness Control: We offer SCD wafers with thicknesses ranging from 0.1 µm up to 500 µm, allowing researchers to optimize the starting material for precise near-surface NV placement and deep etching (600 nm pedestal) requirements.
Customization Potential
Section titled “Customization Potential”The complexity of integrated quantum circuits demands highly customized material preparation, which 6CCVD provides:
| Research Requirement | 6CCVD Customization Service | Benefit to Client |
|---|---|---|
| Scaling Chip Dimensions | Large-Area Wafers: We supply SCD plates up to 10 mm thick and Polycrystalline Diamond (PCD) wafers up to 125 mm in diameter. | Enables the transition from 2 mm x 2 mm lab chips to wafer-scale fabrication, maximizing yield and throughput. |
| Deep Etching into Diamond | Thick Substrates: Provision of robust SCD substrates (up to 10 mm) capable of withstanding the 600 nm RIE pedestal etch and subsequent processing steps. | Ensures mechanical stability and consistency across large-area devices. |
| Integration of Control Electronics | Custom Metalization: In-house deposition of Au, Pt, Pd, Ti, W, and Cu. | Facilitates the integration of electrodes for Stark tuning (required for dynamic stabilization of optical resonances) and RF antennas for spin manipulation, as noted in the paper’s future work section. |
| Surface Quality for GaP Transfer | Ultra-Low Roughness Polishing: SCD polishing to Ra < 1 nm. | Minimizes interface defects and scattering losses, which is crucial for maintaining the high Q factors (up to 11,700) demonstrated in the resonators. |
Engineering Support
Section titled “Engineering Support”6CCVD’s in-house PhD team can assist with material selection and optimization for similar NV Center-Based Quantum Photonic projects. Our expertise covers:
- Substrate Optimization: Consulting on diamond surface termination and cleaning protocols to ensure optimal adhesion and quality for the GaP membrane transfer process.
- Defect Engineering: Guidance on selecting the appropriate diamond grade and thickness to maximize NV center yield and coherence time following implantation and annealing.
- Process Integration: Support for integrating custom metal layers necessary for electro-optic switching (leveraging GaP’s second-order non-linearity) and RF control elements.
For custom specifications or material consultation, visit 6ccvd.com or contact our engineering team directly.
View Original Abstract
We present chip-scale transmission measurements for three key components of a\nGaP-on-diamond integrated photonics platform: waveguide-coupled disk\nresonators, directional couplers, and grating couplers. We also present\nproof-of-principle measurements demonstrating nitrogen-vacancy (NV) center\nemission coupled into selected devices. The demonstrated device performance,\nuniformity and yield place the platform in a strong position to realize\nmeasurement-based quantum information protocols utilizing the NV center in\ndiamond.\n