Charge multiplication effect in thin diamond films
At a Glance
Section titled “At a Glance”| Metadata | Details |
|---|---|
| Publication Date | 2016-07-25 |
| Journal | Applied Physics Letters |
| Authors | N. Skukan, Veljko Grilj, I. Sudić, M. Pomorski, Wataru Kada |
| Institutions | National Institutes for Quantum Science and Technology, Japan Atomic Energy Agency |
| Citations | 19 |
| Analysis | Full AI Review Included |
Executive Summary
Section titled “Executive Summary”- Breakthrough Observation: First reproducible observation of charge multiplication (avalanche effect) in intrinsic single crystal CVD (scCVD) diamond, detected under 18 MeV O ion irradiation.
- Device Architecture: Ultrathin diamond membrane detector (3.25 µm and 4.25 µm thicknesses) with cross-like parallel plate geometry (300×300 µm2 contact overlap).
- Electric Field Regime: Operated at extreme fields from ±500 V (154 V/µm) up to ±650 V (~200 V/µm), far exceeding the conventional operating range of <10 V/µm for diamond radiation detectors.
- Multiplication Factor: Peak charge collection efficiency (CCE) reached 220% at 185 V/µm, corresponding to an ionization coefficient α ≈ 1910 cm-1.
- Predicted Breakdown Threshold: Geiger-mode avalanche threshold extrapolated at 285-363 V/µm depending on fitting model (Chynoweth two-parameter vs. extended three-parameter).
- Fast Transit Times: Intrinsic charge transit time <40 ps; signal rise times ~170 ps (2 GHz bandwidth), demonstrating sub-nanosecond avalanche process and excluding photoconductive gain.
- Application Impact: Enables high signal-to-noise ratio timing detectors, visible-light-beam hardening sensors, and next-generation radiation-hard devices.
Technical Specifications
Section titled “Technical Specifications”| Parameter | Value | Unit | Context |
|---|---|---|---|
| Diamond material | Intrinsic scCVD (Element Six) | — | <1 ppm N, <1 0 0> oriented |
| Detector thickness | 3.25 ± 0.1 | µm | Primary membrane |
| Secondary detector thickness | 4.25 ± 0.3 | µm | Remetallized after breakdown |
| Active contact area | 300 × 300 | µm2 | Cross-like parallel plate overlap |
| Electrode material | Al (sputtered) | — | 300 µm wide strip |
| Wire bond | 60 µm Au wire + Ag-loaded paste | — | To SMA central pin |
| Capacitance | <0.5 | pF | Calculated |
| Leakage current | <100 | fA | Up to ±500 V |
| Operating bias | -640 to +650 | V | ~200 V/µm peak |
| Hard breakdown voltage | -650 | V | Caused microscopic bulk damage |
| Multiplication region field | 30-200 | V/µm | Exponential CCE rise |
| CCE at 100 V (30 V/µm) | 100 | % | Reference plateau |
| CCE at 600 V (185 V/µm) | 220 | % | Charge multiplication peak |
| Ionization coefficient α | 1910 | cm-1 | At 200 V/µm |
| Charge per ion (18 MeV O) | ~830,000 e-h pairs (~133 fC) | — | SRIM simulation |
| Ionizing radiation | 18 MeV O (oxygen ions) | — | Traverses entire membrane |
| Intrinsic transit time | <40 | ps | For 4.25 µm drift path |
| Signal rise time (10-90%) | ~170 | ps | 2 GHz bandwidth |
| Oscilloscope bandwidth | 5 | GHz | 20 Gs/s Lecroy WaveMaster 8500 |
| Geiger threshold (c=1 fit) | 363 | V/µm | Two-parameter Chynoweth |
| Geiger threshold (c=0.2 fit) | 285 | V/µm | Three-parameter extended fit |
| Electron-hole pair creation energy | 13 | eV | Diamond |
| Charge carrier saturation velocity | 1.2-2.7 × 107 | cm/s | Both carriers |
| Beam current (IBIC) | 100-1000 | cps | Low-current mode |
Key Methodologies
Section titled “Key Methodologies”- Starting Material: Standard grade (<1 ppm N) single crystal CVD diamond, <1 0 0> oriented, procured from Element Six.
- Mechanical Pre-thinning: Diamond polished to 30 µm plate by Almax EasyLab.
- Membrane Fabrication: Ar/O plasma etching of central region down to ~3 µm (technique detailed in Pomorski et al., APL 103, 112106, 2013).
- Defect Inspection: Optical microscopy with birefringence imaging to identify bulk- and surface-defect-free membrane zones prior to electrode deposition.
- Electrode Patterning: 300 µm wide Al strip electrodes sputtered on both sides of membrane in cross-like geometry (300×300 µm2 overlap).
- PCB Integration: Sample glued to custom PCB with central via-hole for transmission detection; SMA connector bonded with 60 µm Au wire.
- I-V Pre-screening: Dark current verification (<100 fA up to ±500 V) to confirm dielectric integrity before irradiation.
- Ion Beam Characterization: Thickness confirmed via energy-loss measurements using Si surface barrier ΔE-E telescope; 3.25 ± 0.1 µm thickness derived.
- IBIC Mapping: Charge collection efficiency mapped at 100-1000 cps with Ortec 142A preamplifier + Ortec 570 shaping amplifier + Canberra 8075 ADC.
- Irradiation Source: 18 MeV O ions from RBI ion microprobe; selected for full traversal, homogeneous energy deposition (~10.78 MeV in 3.25 µm), and ~830,000 e-h pairs per ion.
- Charge Sensitive Measurement: Bias swept from -640 to +650 V; Gaussian fitting of spectra normalized to CCE using 13 eV e-h pair creation energy.
- Transient Current Technique (TCT): Bias-tee + Lecroy WaveMaster 8500 (5 GHz, 20 Gs/s) for sub-nanosecond avalanche confirmation; bias limited to 300 V to prevent further breakdown.
- Multiplication Modeling: CCE fitted using both Chynoweth (α = a·exp(-b/E)) and extended Chynoweth (α = a·exp(-(b/E)c)) equations.
6CCVD Solutions & Capabilities
Section titled “6CCVD Solutions & Capabilities”Applicable Materials: Replicating this research requires Optical Grade Single Crystal Diamond (SCD) membranes in the 3-5 µm thickness range with ultra-low nitrogen content (<1 ppm). 6CCVD’s CVD growth capability supports thin-membrane SCD fabrication across the full 0.1 µm - 500 µm thickness spectrum, with substrates available up to 125 mm for polycrystalline formats. For extended studies of impact ionization across thicker geometries or alternative crystal orientations, our polycrystalline diamond (PCD) or tailored SCD plates offer additional flexibility.
Customization Potential:
| Research Requirement | 6CCVD Capability |
|---|---|
| Ultrathin SCD membranes (3-4 µm) | Custom SCD thickness down to 0.1 µm |
| Minimal active contact area (300×300 µm2) | Laser cutting service for arbitrary geometry definition |
| Al electrode metallization | Internal custom metallization with Au, Pt, Pd, Ti, W, or Cu |
| Defect-region avoidance | Birefringence-grade inspection; Ra < 1 nm polished SCD surfaces |
| Capacitance minimization via small contact | Custom electrode patterning via shadow mask or photolithography-compatible metallization |
| Membrane thinning (Ar/O plasma etching ready) | Delivery of pre-thinned membranes or thicker plates suitable for downstream etching |
Engineering Support: 6CCVD’s in-house PhD engineering team routinely supports radiation detection, particle physics, and quantum sensing programs. We can assist in:
- Selecting optimal SCD grade (electronic vs. optical vs. boron-doped) for impact ionization studies.
- Defining electrode stacks (e.g., Ti/Pt/Au for harsh environments or pure Al for low-leakage thin-film work).
- Recommending thickness/membrane configurations to balance breakdown strength with charge yield.
- Co-developing TCT- or IBIC-ready detector prototypes.
This research aligns with 6CCVD’s strengths in sub-10 µm diamond membranes, low-leakage contact engineering, and radiation-hard detector prototyping—making us a natural partner for next-generation avalanche-mode diamond sensors, high-field device characterization, and ATLAS/CMS-class detector development.
Call to Action: For custom specifications, membrane prototyping, or material consultation on charge multiplication and high-field diamond detector projects, visit 6ccvd.com or contact our engineering team directly.
View Original Abstract
Herein, we report on the enhanced sensitivity for the detection of charged particles in single crystal chemical vapour deposition (scCVD) diamond radiation detectors. The experimental results demonstrate charge multiplication in thin planar diamond membrane detectors, upon impact of 18 MeV O ions, under high electric field conditions. Avalanche multiplication is widely exploited in devices such as avalanche photo diodes, but has never before been reproducibly observed in intrinsic CVD diamond. Because enhanced sensitivity for charged particle detection is obtained for short charge drift lengths without dark counts, this effect could be further exploited in the development of sensors based on avalanche multiplication and radiation detectors with extreme radiation hardness.