Skip to content

Dielectric charging phenomena in diamond films used in RF MEMS capacitive switches - The effect of film thickness

MetadataDetails
Publication Date2016-09-01
JournalMicroelectronics Reliability
AuthorsM. Koutsoureli, A. Zevgolatis, S. Saada, Christine Mer-Calfati, L. Michalas
InstitutionsCommissariat à l’Énergie Atomique et aux Énergies Alternatives, National and Kapodistrian University of Athens
Citations2
AnalysisFull AI Review Included

Technical Analysis: RF MEMS Reliability Improvement via Nanocrystalline Diamond Thickness Control

Section titled “Technical Analysis: RF MEMS Reliability Improvement via Nanocrystalline Diamond Thickness Control”

Document Prepared For: Engineers and Scientists specializing in RF Microelectromechanical Systems (MEMS), Wide Bandgap Semiconductors, and High-Reliability Dielectrics.

Source Analysis: Dielectric charging phenomena in diamond films used in RF MEMS capacitive switches: The effect of film thickness


This paper investigates the critical role of film thickness in mitigating dielectric charging—a primary failure mechanism—in Nanocrystalline Diamond (NCD) films utilized in RF MEMS capacitive switches.

  • Core Finding: Thinner NCD films significantly enhance the reliability of RF MEMS switches by reducing overall dielectric charging and lowering defect density.
  • Optimal Thickness: Films at 350 nm thickness exhibited the lowest conductivity and stored charge density (4.71 x 10-6 C/cm2).
  • Conduction Mechanisms Identified: Current transport varies significantly based on field intensity: thermally activated hopping (low fields, < 130 kV/cm) transitions to Hill-modified Frenkel-Poole conduction (high fields, > 130 kV/cm).
  • Defect Correlation: Increasing film thickness correlates directly with increased conductivity and higher defect density (N), suggesting a less desirable grain boundary structure in thicker films.
  • Charging Mechanism: Thermally Stimulated Depolarization Current (TSDC) analysis confirmed that charges are trapped within the material’s volume, emphasizing the importance of high-quality internal morphology.
  • 6CCVD Relevance: The research confirms the necessity of high-precision MPCVD synthesis and rigorous thickness control in Polycrystalline Diamond (PCD) films for commercialization of high-performance RF MEMS devices.

Extracted quantitative data points relating NCD film thickness to key electrical properties.

Parameter350 nm Film Value750 nm Film ValueUnitContext
Growth Temperature1023 K (750 °C)1023 K (750 °C)KMPCVD Substrate Temperature
Low Field Intensity Threshold130kV/cmElectric FieldTransition point for conduction mechanism
Low Field Activation Energy (EA)0.82 ± 0.020.66 ± 0.02eVThermally activated conduction (< 130 kV/cm)
High Field Activation Energy (Ei)0.84 ± 0.020.95 ± 0.01eVHill Conduction mechanism (> 130 kV/cm)
Mean Hopping Distance (s)52.3 ± 2.628.8 ± 0.5nmDecreases with increasing thickness
Density of Centers (N)(7.0 ± 1.0) x 1015(4.2 ± 0.2) x 1016cm-3Increases significantly with thickness (Defect Density)
Total Stored Charge (σTSDC)(4.71 ± 0.07) x 10-6(7.94 ± 0.06) x 10-6C/cm2Dielectric Charging Metric (Lower is better)
Capacitor Area450 x 450µm2AreaUtilized MIM capacitor test structure
TSDC Temperature Range200 - 450KTemperatureRange for depolarization current measurement

The researchers fabricated Metal-Insulator-Metal (MIM) capacitors using NCD films deposited via Microwave Plasma Assisted Chemical Vapor Deposition (MPCVD).

  1. Substrate Preparation: Silicon wafers were utilized, topped with an electrode stack of TiW/Au.
  2. Nanoseeding: A proprietary nanoseeding technique (diamond nanocrystals dispersed in Polyvinyl Alcohol, PVA, via spin coating) was used to achieve high nucleation density and ensure a continuous diamond film.
  3. MPCVD Growth Conditions:
    • Reactor Type: Home-made designed MPCVD system (2.45 GHz-2 kW SAIREM generator).
    • Base Pressure: Approximately 10-6 mbar.
    • Gas Mixture: 0.6% Methane (CH4) diluted in Hydrogen (H2).
    • Total Pressure: 35 mbar.
    • Microwave Power: 900 W.
    • Substrate Temperature: Maintained at 1023 K (750 °C).
  4. Thickness Control: Film thickness was monitored in situ using a home-made laser interferometry system to stop growth precisely at the target thicknesses (350 nm, 600 nm, 750 nm).
  5. Characterization:
    • I-V/Conductivity: Measured in a vacuum cryostat (Pressure ~ 10-3 Torr) between 300 K and 400 K using a Keithley 6487.
    • Dielectric Charging: Investigated using Thermally Stimulated Depolarization Currents (TSDC) technique (200 K-450 K, 2.5 K/min heating rate).

This research validates the critical requirement for precise thickness control and high-quality MPCVD diamond material for achieving reliable RF MEMS dielectrics. 6CCVD is uniquely positioned to supply materials that meet or exceed these specifications, offering superior process control for next-generation diamond-based devices.

The research utilizes nanocrystalline diamond (NCD), which is a key variant of Polycrystalline Diamond (PCD).

Application Requirement6CCVD Material RecommendationTechnical Advantage
RF MEMS DielectricOptical Grade PCD (Polycrystalline Diamond)Extremely low loss tangent (tan δ) and high dielectric strength required for RF applications.
Precise Thin FilmsPCD or NCD (Sub-micron thickness)6CCVD offers PCD down to 0.1 µm (100 nm), allowing replication of the highly reliable 350 nm films or exploration of even thinner layers for improved performance (higher isolation, increased down-state capacitance).
Substrate CompatibilityCustom Substrate Bonding ServicesAbility to grow NCD/PCD directly on Si, SiO2, or handle the required TiW/Au/Si stacks used in the paper.

The MIM structure and precise electrode definition are central to this research. 6CCVD provides comprehensive manufacturing capabilities to support direct replication or advanced modification of this architecture.

  • Precision Thickness Control: We routinely manage diamond film thickness across large wafers (up to 125mm) with the high uniformity necessary for reproducible electrical performance in the critical sub-micron range (0.1 µm to 500 µm).
  • Custom Micro-Patterning: For the utilized 450 x 450 µm2 capacitor area, 6CCVD offers high-resolution laser cutting and etching services to define structures far below the inch scale.
  • Integrated Metallization: The paper required TiW/Au contacts. 6CCVD provides internal metalization capabilities, including Au, Pt, Pd, Ti, W, and Cu, allowing researchers to test various electrode materials known to influence charge injection and trapping.
  • Surface Finish: Maintaining the lowest possible surface roughness is critical for highly uniform thin films. 6CCVD guarantees surface polishing down to Ra < 5 nm for inch-size PCD wafers, ensuring optimal interface quality for reduced defect generation.

The findings regarding the correlation between film thickness, defect density (N), and activation energy (Ei/EA) provide a clear roadmap for material optimization.

6CCVD’s in-house PhD team provides authoritative engineering consultation to assist clients in selecting optimal MPCVD parameters (e.g., CH4 concentration, pressure, and temperature) to achieve the lowest possible sp2/sp3 ratio and lowest defect density (N) necessary for high-reliability RF MEMS capacitive switches and similar high-frequency dielectric applications.